Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | O | EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755 | ||
20.0 °C | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 100.0 MPa Show Material materials with Bending Fatigue Strength of 100.0 MPa | O | EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755 | |||
Biegewinkel 180° | 0.5 °/t Show Material materials with Biegewinkel 180° of 0.5 °/t | O | EN 573-3, EN 485 | |||
Biegewinkel 90° | 0.5 °/t Show Material materials with Biegewinkel 90° of 0.5 °/t | O | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | O | EN 573-3, EN 485 | ||||
2.0 °/t Show Material materials with Biegewinkel 90° of 2.0 °/t | O | EN 573-3, EN 485 | ||||
Dehnung | 13.0 % Show Material materials with Dehnung of 13.0 % | O | EN 573-3, EN 1396, EN 485 | A50 | ||
14.0 % Show Material materials with Dehnung of 14.0 % | O | EN 573-3, EN 1396, EN 485 | A50 | |||
15.0 % Show Material materials with Dehnung of 15.0 % | O | EN 573-3, EN 1301 | ||||
15.0 % Show Material materials with Dehnung of 15.0 % | O | EN 573-3, EN 754, EN 755 | A50 | |||
16.0 % Show Material materials with Dehnung of 16.0 % | O | EN 573-3, EN 1396, EN 485 | A50 | |||
17.0 % Show Material materials with Dehnung of 17.0 % | O | EN 573-3, EN 754, EN 755 | A100 | |||
18.0 % Show Material materials with Dehnung of 18.0 % | O | EN 573-3, EN 485 | A100 | |||
18.0 % Show Material materials with Dehnung of 18.0 % | O | EN 573-3, EN 485 | A50 | |||
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Wire | A100 | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Wire | A10 | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube | A10 | |
20.0 °C | 17.0 % Show Material materials with Dehnung of 17.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | A10 | |
20.0 °C | 17.0 % Show Material materials with Dehnung of 17.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube | ||
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | O | EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755 | |||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire | ||
Härte, Brinell | 44.0 [-] Show Material materials with Härte, Brinell of 44.0 [-] | O | EN 573-3, EN 485 | |||
20.0 °C | 40.0 [-] Show Material materials with Härte, Brinell of 40.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube, Wire | ||
20.0 °C | 45.0 [-] Show Material materials with Härte, Brinell of 45.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Schubmodule | 26.3 GPa Show Material materials with Schubmodule of 26.3 GPa | O | EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755 | |||
20.0 °C | 26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire | ||
Zugfestigkeit | 150.0 - 200.0 MPa Show Material materials with Zugfestigkeit of 150.0 - 200.0 MPa | O | EN 573-3, EN 754 | |||
160.0 - 200.0 MPa Show Material materials with Zugfestigkeit of 160.0 - 200.0 MPa | O | EN 573-3, EN 1396, EN 485 | ||||
160.0 - 220.0 MPa Show Material materials with Zugfestigkeit of 160.0 - 220.0 MPa | O | EN 573-3, EN 755 | ||||
215.0 MPa Show Material materials with Zugfestigkeit of 215.0 MPa | O | EN 573-3, EN 1301 | ||||
20.0 °C | 150.0 MPa Show Material materials with Zugfestigkeit of 150.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Tube, Wire | ||
20.0 °C | 155.0 - 200.0 MPa Show Material materials with Zugfestigkeit of 155.0 - 200.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3699999999999997e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755 | ||
100 °C | 2.3699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3699999999999997e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755 | |||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 610.0 - 650.0 °C Show Material materials with Schmelzpunkt of 610.0 - 650.0 °C | O | EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755 | |||
Spezifische Wärmekapazität | 20.0 °C | 921.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 921.0 J/(kg·K) | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire | |
Wärmeleitfähigkeit | 140.0 - 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 140.0 - 160.0 W/(m·K) | O | EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755 | |||
20.0 °C | 167.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 167.0 W/(m·K) | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 25000000.0 - 30000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 25000000.0 - 30000000.0 S/m | O | EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755 | ||
20.0 °C | 26000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 26000000.0 S/m | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire | |
spezifischer Widerstand | 3.33e-08 - 4e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.33e-08 - 4e-08 Ω·m | O | EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.15 % Show Material materials with Chrom of 0.15 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 485, EN 754, EN 755 | Rod, Sheet, Strip, Tube, Wire |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Rod, Sheet, Strip, Tube, Wire |
0.50 % Show Material materials with Eisen of 0.50 % | O | EN 573-3, EN 1301, EN 1396, EN 485, EN 754, EN 755 | ||
Kupfer | 0.15 % Show Material materials with Kupfer of 0.15 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 485, EN 754, EN 755 | Rod, Sheet, Strip, Tube, Wire |
Magnesium | 1.7 - 2.4 % Show Material materials with Magnesium of 1.7 - 2.4 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 485, EN 754, EN 755 | Rod, Sheet, Strip, Tube, Wire |
Mangan | 0.1 - 0.5 % Show Material materials with Mangan of 0.1 - 0.5 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 485, EN 754, EN 755 | Rod, Sheet, Strip, Tube, Wire |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 485, EN 754, EN 755 | Rod, Sheet, Strip, Tube, Wire |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 485, EN 754, EN 755 | Rod, Sheet, Strip, Tube, Wire |
Zink | 0.15 % Show Material materials with Zink of 0.15 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 485, EN 754, EN 755 | Rod, Sheet, Strip, Tube, Wire |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): sufficient / poor, friction soldering: good, soft brazing with flux: sufficient | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / acceptable (H12) |