Allgemein
Property | Value | Condition | Related Standards |
---|---|---|---|
Dichte | 2.85 g/cm³ Show Material materials with Dichte of 2.85 g/cm³ | T4 | EN 573-3, EN 755 |
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Elastizitätsmodul | 72.5 GPa Show Material materials with Elastizitätsmodul of 72.5 GPa | T4 | EN 573-3, EN 755 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||
Schubmodule | 27.3 GPa Show Material materials with Schubmodule of 27.3 GPa | T4 | EN 573-3, EN 755 | |
Zugfestigkeit | 330.0 MPa Show Material materials with Zugfestigkeit of 330.0 MPa | T4 | EN 573-3, EN 755 | |
340.0 MPa Show Material materials with Zugfestigkeit of 340.0 MPa | T4 | EN 573-3, EN 755 | ||
370.0 MPa Show Material materials with Zugfestigkeit of 370.0 MPa | T4 | EN 573-3, EN 755 |
Thermisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T4 | EN 573-3, EN 755 |
100 °C | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T4 | EN 573-3, EN 755 | |
Schmelzpunkt | 507.0 - 650.0 °C Show Material materials with Schmelzpunkt of 507.0 - 650.0 °C | T4 | EN 573-3, EN 755 | |
Spezifische Wärmekapazität | 860.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 860.0 J/(kg·K) | T4 | EN 573-3, EN 755 | |
Wärmeleitfähigkeit | 130.0 - 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 160.0 W/(m·K) | T4 | EN 573-3, EN 755 |
Elektrisch
Property | Value | Condition | Related Standards |
---|---|---|---|
Elektrische Leitfähigkeit | 18000000.0 - 22000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 22000000.0 S/m | T4 | EN 573-3, EN 755 |
spezifischer Widerstand | 4.55e-08 - 5.56e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.55e-08 - 5.56e-08 Ω·m | T4 | EN 573-3, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Bismut | 0.2 % Show Material materials with Bismut of 0.2 % | T4 | EN 573-3, EN 755 |
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | T4 | EN 573-3, EN 755 |
Eisen | 0.80 % Show Material materials with Eisen of 0.80 % | T4 | EN 573-3, EN 755 |
Kupfer | 3.3 - 4.6 % Show Material materials with Kupfer of 3.3 - 4.6 % | T4 | EN 573-3, EN 755 |
Magnesium | 0.4 - 1.8 % Show Material materials with Magnesium of 0.4 - 1.8 % | T4 | EN 573-3, EN 755 |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | T4 | EN 573-3, EN 755 |
Nickel | 0.2 % Show Material materials with Nickel of 0.2 % | T4 | EN 573-3, EN 755 |
Silizium | 0.8 % Show Material materials with Silizium of 0.8 % | T4 | EN 573-3, EN 755 |
Titan | 0.2 % Show Material materials with Titan of 0.2 % | T4 | EN 573-3, EN 755 |
Zink | 0.8 % Show Material materials with Zink of 0.8 % | T4 | EN 573-3, EN 755 |
Zinn | 0.2 % Show Material materials with Zinn of 0.2 % | T4 | EN 573-3, EN 755 |
Technological properties
Property | ||
---|---|---|
Anodizing | Protective: poor | |
Brazing | friction soldering: sufficient | |
Corrosion properties | Seawater: poor, weathering: poor | |
Workability | Bending / Spinning (cold): sufficient / -, Deep drawing / upsetting (Condition) - / sufficient |