Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 8.3 g/cm³ Show Material materials with Dichte of 8.3 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 23.0 °C | 25 % Show Material materials with Dehnung of 25 % | |
Elastizitätsmodul | 23.0 °C | 100 - 125 GPa Show Material materials with Elastizitätsmodul of 100 - 125 GPa | Typical for Wrought Copper Brass |
Härte, Vickers | 23.0 °C | 110 [-] Show Material materials with Härte, Vickers of 110 [-] | |
Schubmodule | 23.0 °C | 40 GPa Show Material materials with Schubmodule of 40 GPa | Typical for Wrought Copper Brass |
Streckgrenze Rp 0,2 | 23.0 °C | 140 MPa Show Material materials with Streckgrenze Rp 0,2 of 140 MPa | |
Zugfestigkeit | 23.0 °C | 390 MPa Show Material materials with Zugfestigkeit of 390 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.7E-5 - 2.1E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 - 2.1E-5 1/K | Typical for Wrought Copper Brass |
Schmelzpunkt | 875 - 1075 °C Show Material materials with Schmelzpunkt of 875 - 1075 °C | Typical for Wrought Copper Brass | |
Spezifische Wärmekapazität | 23.0 °C | 371 - 418 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 371 - 418 J/(kg·K) | Typical for Wrought Copper Brass |
Wärmeleitfähigkeit | 23.0 °C | 100 - 234 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 100 - 234 W/(m·K) | Typical for Wrought Copper Brass |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.1 - 0.5 % Show Material materials with Aluminium of 0.1 - 0.5 % |
Andere | Rest Zn, total 0.2 |
Arsen | 0.05 % Show Material materials with Arsen of 0.05 % |
Blei | 0.3 - 0.7 % Show Material materials with Blei of 0.3 - 0.7 % |
Eisen | 0.1 - 0.4 % Show Material materials with Eisen of 0.1 - 0.4 % |
Kupfer | 59 - 60.7 % Show Material materials with Kupfer of 59 - 60.7 % |
Nickel | 0.2 - 0.5 % Show Material materials with Nickel of 0.2 - 0.5 % |
Zinn | 0.3 - 0.7 % Show Material materials with Zinn of 0.3 - 0.7 % |