Property | Value | Comment | |
---|---|---|---|
Carbon equivalent (CEV) | 0.43 [-] Show Supplier Material materials with Carbon equivalent (CEV) of 0.43 [-] | Cast | |
Carbon equivalent note | CEV = C + Mn/6 + (Cr+Mo+V)/5 + (Cu+Ni)/15 and PCM = C + Si/30 + (Cr+Mn+Cu)/20 + Ni/60 + Mo/15 + V/10 + 5B |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 22 % Show Supplier Material materials with Dehnung of 22 % | min. A5.65√So | for thickness 5-40 mm | Transverse | |
Kerbschlagenergie | -40 °C | 50 J Show Supplier Material materials with Kerbschlagenergie of 50 J | min. | for thickness 5-40 mm |
Streckgrenze | 345 MPa Show Supplier Material materials with Streckgrenze of 345 MPa | min. | for thickness 16-40 mm | Transverse | |
355 MPa Show Supplier Material materials with Streckgrenze of 355 MPa | min. | for thickness 5-16 mm | Transverse | ||
Zugfestigkeit | 470 - 630 MPa Show Supplier Material materials with Zugfestigkeit of 470 - 630 MPa | for thickness 5-40 mm | Transverse |
Chemical properties
Property | Value | Comment |
---|---|---|
Aluminium | 0.02 % Show Supplier Material materials with Aluminium of 0.02 % | min. | for thickness 5-40 mm |
Chrom | 0.3 % Show Supplier Material materials with Chrom of 0.3 % | max. | for thickness 5-40 mm |
Kohlenstoff | 0.18 % Show Supplier Material materials with Kohlenstoff of 0.18 % | max. | for thickness 5-40 mm |
Kupfer | 0.35 % Show Supplier Material materials with Kupfer of 0.35 % | max. | for thickness 5-40 mm |
Mangan | 0.9 - 1.65 % Show Supplier Material materials with Mangan of 0.9 - 1.65 % | for thickness 5-40 mm |
Molybdän | 0.1 % Show Supplier Material materials with Molybdän of 0.1 % | max. | for thickness 5-40 mm |
Nickel | 0.5 % Show Supplier Material materials with Nickel of 0.5 % | max. | for thickness 5-40 mm |
Niobium | 0.06 % Show Supplier Material materials with Niobium of 0.06 % | max. | for thickness 5-40 mm |
Phosphor | 0.03 % Show Supplier Material materials with Phosphor of 0.03 % | max. | for thickness 5-40 mm |
Schwefel | 0.025 % Show Supplier Material materials with Schwefel of 0.025 % | max. | for thickness 5-40 mm |
Silizium | 0.5 % Show Supplier Material materials with Silizium of 0.5 % | max. | for thickness 5-40 mm |
Stickstoff | 0.015 % Show Supplier Material materials with Stickstoff of 0.015 % | max. | for thickness 5-40 mm |
Titan | 0.03 % Show Supplier Material materials with Titan of 0.03 % | max. | for thickness 5-40 mm |
Vanadium | 0.12 % Show Supplier Material materials with Vanadium of 0.12 % | max. | for thickness 5-40 mm |
Technological properties
Property | ||
---|---|---|
Application areas | Offshore structures such as platforms and equipment for new offshore windmill towers. | |
Chemical composition | The above chemical properties are based on cast analysis data. Product analysis may be requested at the time of order. | |
Delivery condtion | For the dimensions available please visit Dimension tables (see Table A). Table A with a thickness range as indicated in the Mechanical properties. | |
Other | Available options Options available (after previous agreement): |