Property | Value | Testing Standard | Condition | Comment |
---|---|---|---|---|
Dichte | 1.78 - 1.82 g/cm³ Show Supplier Material materials with Dichte of 1.78 - 1.82 g/cm³ | ASTM D792 | ||
Sauerstoffindex | 42 % Show Supplier Material materials with Sauerstoffindex of 42 % | ASTM D2863 | ||
45 % Show Supplier Material materials with Sauerstoffindex of 45 % | ISO 4589-1/-2 | dry | ||
Wasserabsorption | 0.5 % Show Supplier Material materials with Wasserabsorption of 0.5 % | ASTM D570 | max. |
Mechanisch
Property | Value | Testing Standard | Condition | Comment |
---|---|---|---|---|
Biegemodul | 0.241 - 0.379 GPa Show Supplier Material materials with Biegemodul of 0.241 - 0.379 GPa | ASTM D790 | ||
Dehnung | 50 % Show Supplier Material materials with Dehnung of 50 % | ISO 527-1/-2 | dry | min. | nominal |
500 % Show Supplier Material materials with Dehnung of 500 % | ASTM D638 | min. | ||
Elastizitätsmodul | 0.207 - 0.345 GPa Show Supplier Material materials with Elastizitätsmodul of 0.207 - 0.345 GPa | ASTM D638 | ||
0.283 GPa Show Supplier Material materials with Elastizitätsmodul of 0.283 GPa | ISO 527-1/-2 | dry | ||
Elongation at yield | 25 - 40 % Show Supplier Material materials with Elongation at yield of 25 - 40 % | ASTM D638 | ||
30 % Show Supplier Material materials with Elongation at yield of 30 % | ISO 527-1/-2 | dry | ||
Härte, Shore D | 45 - 55 [-] Show Supplier Material materials with Härte, Shore D of 45 - 55 [-] | ASTM D2240 | ||
Impact strength, Charpy notched, ASTM | No Break at 23°C | ASTM D256 | ||
Schlagfestigkeit, Charpy gekerbt | No Break at 23°C | ISO 179/1eA | dry | |
Streckgrenze | 12.4 - 16.5 MPa Show Supplier Material materials with Streckgrenze of 12.4 - 16.5 MPa | ASTM D638 | ||
Zugfestigkeit | 19.3 - 24.8 MPa Show Supplier Material materials with Zugfestigkeit of 19.3 - 24.8 MPa | ASTM D638 |
Thermisch
Property | Value | Condition | Testing Standard | Comment | |||
---|---|---|---|---|---|---|---|
Glasübergangstemperatur | -42 °C Show Supplier Material materials with Glasübergangstemperatur of -42 °C | dry | ISO 11357-1/-2 | 10°C/min | |||
-40 °C Show Supplier Material materials with Glasübergangstemperatur of -40 °C | ASTM D7028 | ||||||
Koeffizient der thermischen Ausdehnung | 0.000153 - 0.000194 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 0.000153 - 0.000194 1/K | ASTM D696 | |||||
Schmelzpunkt | 160 - 168 °C Show Supplier Material materials with Schmelzpunkt of 160 - 168 °C | ASTM D3418 | |||||
164 °C Show Supplier Material materials with Schmelzpunkt of 164 °C | dry | ISO 11357-1/-3 | 10°C/min | ||||
Entflammbarkeit | At thickness 0.8 mm IEC 60695-11-10: V-0 |
Elektrisch
Property | Value | Testing Standard | Condition |
---|---|---|---|
Durchschlagfestigkeit | 39.4 - 47.2 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 39.4 - 47.2 kV/mm | ASTM D149 | |
Surface resistivity | 7.6e+11 - 7.8e+11 Ω/sq Show Supplier Material materials with Surface resistivity of 7.6e+11 - 7.8e+11 Ω/sq | ASTM D257 | |
Volume resistivity | 2e+14 Ω·cm Show Supplier Material materials with Volume resistivity of 2e+14 Ω·cm | IEC 60093 | dry |
Rheological Properties
Property | Value | Testing Standard | Comment |
---|---|---|---|
Melt viscosity | 700 - 1300 Pa·s Show Supplier Material materials with Melt viscosity of 700 - 1300 Pa·s | ASTM D3835 | |
Schmelzmassenflussrate | 8 - 25 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 8 - 25 g/10min | ASTM D1238 | 230°C/3.8kg |
Technological properties
Property | ||
---|---|---|
Application areas | Automotive Cables,Foamed PVDF Cable Jacketing,Performance Wire,PVDF Cable Jacketing,Wire and Cables |