Allgemein
Property | Value | Testing Standard | Condition | Comment |
---|---|---|---|---|
Coefficient of friction | 0.14 [-] Show Supplier Material materials with Coefficient of friction of 0.14 [-] | ASTM D1894 | vs Steel, Kinetic | |
0.2 [-] Show Supplier Material materials with Coefficient of friction of 0.2 [-] | ASTM D1894 | vs Steel, Static | ||
Dichte | 1.77 - 1.79 g/cm³ Show Supplier Material materials with Dichte of 1.77 - 1.79 g/cm³ | ASTM D792 | ||
1.78 g/cm³ Show Supplier Material materials with Dichte of 1.78 g/cm³ | ISO 1183 | dry | ||
Sauerstoffindex | 43 % Show Supplier Material materials with Sauerstoffindex of 43 % | ISO 4589-1/-2 | dry | |
44 % Show Supplier Material materials with Sauerstoffindex of 44 % | ASTM D2863 | |||
Wasserabsorption | 0.01 - 0.03 % Show Supplier Material materials with Wasserabsorption of 0.01 - 0.03 % | ASTM D570 | ||
0.03 % Show Supplier Material materials with Wasserabsorption of 0.03 % | Sim. to ISO 62 |
Mechanisch
Property | Temperature | Value | Testing Standard | Condition | Comment |
---|---|---|---|---|---|
Biegefestigkeit | 58.6 - 75.8 MPa Show Supplier Material materials with Biegefestigkeit of 58.6 - 75.8 MPa | ASTM D790 | at 5% strain | ||
Biegemodul | 1.4 - 2.3 GPa Show Supplier Material materials with Biegemodul of 1.4 - 2.3 GPa | ASTM D790 | |||
Dehnung | 20 - 100 % Show Supplier Material materials with Dehnung of 20 - 100 % | ASTM D638 | |||
50 % Show Supplier Material materials with Dehnung of 50 % | ISO 527-1/-2 | dry | min. | nominal | ||
Druckfestigkeit | 68.9 - 103 MPa Show Supplier Material materials with Druckfestigkeit of 68.9 - 103 MPa | ASTM D695 | |||
Elastizitätsmodul | 1.4 - 2.3 GPa Show Supplier Material materials with Elastizitätsmodul of 1.4 - 2.3 GPa | ASTM D638 | |||
2.3 GPa Show Supplier Material materials with Elastizitätsmodul of 2.3 GPa | ISO 527-1/-2 | dry | |||
Elongation at yield | 5 - 10 % Show Supplier Material materials with Elongation at yield of 5 - 10 % | ASTM D638 | |||
9 % Show Supplier Material materials with Elongation at yield of 9 % | ISO 527-1/-2 | dry | |||
Härte, Shore D | 76 - 80 [-] Show Supplier Material materials with Härte, Shore D of 76 - 80 [-] | ASTM D2240 | |||
Impact strength, Charpy notched, ASTM | 23 °C | 80.1 - 214 J/m Show Supplier Material materials with Impact strength, Charpy notched, ASTM of 80.1 - 214 J/m | ASTM D256 | ||
Impact strength, Charpy unnotched, ASTM | 23 °C | 1070 - 4270 J/m Show Supplier Material materials with Impact strength, Charpy unnotched, ASTM of 1070 - 4270 J/m | ASTM D256 | ||
Schlagfestigkeit, Charpy gekerbt | -30 °C | 5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 5 kJ/m² | ISO 179/1eA | dry | |
23 °C | 8 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 8 kJ/m² | ISO 179/1eA | dry | ||
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 208 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 208 kJ/m² | ISO 179/1eU | dry | |
23 °C | 192 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 192 kJ/m² | ISO 179/1eU | dry | ||
Streckgrenze | 44.8 - 55.2 MPa Show Supplier Material materials with Streckgrenze of 44.8 - 55.2 MPa | ASTM D638 | |||
54 MPa Show Supplier Material materials with Streckgrenze of 54 MPa | ISO 527-1/-2 | dry | |||
Zugfestigkeit | 34.5 - 55.2 MPa Show Supplier Material materials with Zugfestigkeit of 34.5 - 55.2 MPa | ASTM D638 |
Thermisch
Property | Value | Testing Standard | Condition | Pressure | Comment | ||||
---|---|---|---|---|---|---|---|---|---|
Glasübergangstemperatur | -40.6 - -38.3 °C Show Supplier Material materials with Glasübergangstemperatur of -40.6 - -38.3 °C | ASTM D7028 | |||||||
-40 °C Show Supplier Material materials with Glasübergangstemperatur of -40 °C | ISO 11357-1/-2 | dry | 10°C/min | ||||||
Koeffizient der thermischen Ausdehnung | 0.000119 - 0.000144 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 0.000119 - 0.000144 1/K | ASTM D696 | |||||||
0.00015 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 0.00015 1/K | ISO 11359-1/-2 | dry | |||||||
Relative temperature index, electrical | 150 °C Show Supplier Material materials with Relative temperature index, electrical of 150 °C | UL 746B | |||||||
Relative temperature index, mechanical strength | 150 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 150 °C | UL 746B | |||||||
Schmelzpunkt | 165 - 172 °C Show Supplier Material materials with Schmelzpunkt of 165 - 172 °C | ASTM D3418 | |||||||
168 °C Show Supplier Material materials with Schmelzpunkt of 168 °C | ISO 11357-1/-3 | dry | 10°C/min | ||||||
Spezifische Wärmekapazität | 665 - 958 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 665 - 958 J/(kg·K) | DSC | |||||||
Thermal decomposition in air | 375 °C Show Supplier Material materials with Thermal decomposition in air of 375 °C | TGA | 1% wt. loss | ||||||
Thermal decomposition in nitrogen | 410 °C Show Supplier Material materials with Thermal decomposition in nitrogen of 410 °C | TGA | 1% wt. loss | ||||||
Vicat-Erweichungstemperatur | 140 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 140 °C | ISO 306 | 50°C/h 50N | ||||||
Wärmeformbeständigkeitstemperatur | 105 - 115 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 105 - 115 °C | ASTM D648 | 2 MPa | 248 °F/hr | |||||
110 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 110 °C | ISO 75-1/-2 | dry | 2 MPa | ||||||
125 - 140 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 125 - 140 °C | ASTM D648 | 0.45 MPa | 248 °F/hr | ||||||
130 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 130 °C | ISO 75-1/-2 | dry | 0.45 MPa | ||||||
Wärmeleitfähigkeit | 0.17 - 0.19 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 0.17 - 0.19 W/(m·K) | ASTM D433 | |||||||
Entflammbarkeit | At thickness 1.6 mm IEC 60695-11-10: V-0, At thickness 0.8 mm IEC 60695-11-10: V-0 and yellow card available |
Elektrisch
Property | Value | Frequency | Testing Standard | Condition |
---|---|---|---|---|
Dielektrizitätskonstante | 4.5 - 9.5 [-] Show Supplier Material materials with Dielektrizitätskonstante of 4.5 - 9.5 [-] | 1KHz | ASTM D150 | |
6 [-] Show Supplier Material materials with Dielektrizitätskonstante of 6 [-] | 1MHz | IEC 60250 | dry | |
9 [-] Show Supplier Material materials with Dielektrizitätskonstante of 9 [-] | 100Hz | IEC 60250 | dry | |
Durchschlagfestigkeit | 67 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 67 kV/mm | ASTM D149 | ||
Verlustfaktor | 0.01 - 0.21 [-] Show Supplier Material materials with Verlustfaktor of 0.01 - 0.21 [-] | 100KHz | ASTM D150 | |
0.035 [-] Show Supplier Material materials with Verlustfaktor of 0.035 [-] | 100Hz | IEC 60250 | dry | |
0.206 [-] Show Supplier Material materials with Verlustfaktor of 0.206 [-] | 1MHz | IEC 60250 | dry | |
Volume resistivity | 2e+14 Ω·cm Show Supplier Material materials with Volume resistivity of 2e+14 Ω·cm | ASTM D257 | 65% RH | |
2e+14 Ω·cm Show Supplier Material materials with Volume resistivity of 2e+14 Ω·cm | IEC 60093 | dry |
Optisch
Property | Value | Testing Standard | Comment |
---|---|---|---|
Brechungsindex | 1 [-] Show Supplier Material materials with Brechungsindex of 1 [-] | ASTM D542 | sodium D line |
Rheological Properties
Property | Value | Testing Standard | Condition | Comment |
---|---|---|---|---|
Melt viscosity | 400 - 800 Pa·s Show Supplier Material materials with Melt viscosity of 400 - 800 Pa·s | ASTM D3835 | ||
Schmelzmassenflussrate | 19 - 35 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 19 - 35 g/10min | ASTM D1238 | 230°C/3.8kg | |
Schmelzvolumenflussrate | 20 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 20 cm³/10min | ISO 1133 | dry | 230°C/5kg |
Schrumpfung | 2 % Show Supplier Material materials with Schrumpfung of 2 % | ISO 294-4 | dry | |
2 % Show Supplier Material materials with Schrumpfung of 2 % | ISO 294-4 | dry | Transverse |
Technological properties
Property | ||
---|---|---|
Application areas | Chemical Process Industry,Chemical Process Industry - Injection Molding,Tower Packing,Plenum Cable | |
Certifications | Yellow Card | |
Processing methods | Injection Molding: |