1.4501 (X2CrNiMoCuWN25-7-4) is a grade of super-duplex based on 25% chromium, 7% nickel with an addition of tungsten which enhances the pitting index (PREN) even further above the 40 minimum and also contributes to alloy strength. This high resistance to pitting is combined with a high tensile strength and higher resistance to stress corrosion cracking at moderate temperatures to that of conventional austenitic stainless steels. A small addition of copper (lower than in S32550/AMAZON 256) enhances its general corrosion resistance. It shows the following features and properties:


  • Very high strength
  • Very high resistance to pitting
  • Very good corrosion resistance
  • High resistance to erosion and abrasion in flowing systems
  • High resistance to stress corrosion cracking, fatigue and erosion
  • Related Standards

    Equivalent Materials

    Diese Materialdaten wurden von Matmatch zur Verfügung gestellt

    Alle Daten beziehen sich auf Raumtemperatur soweit nicht anderweitig spezifiziert. SI Einheiten werden verwendt soweit nicht anderweitig spezifiziert.
    Äquivalente Standards sind ähnlich zu einem oder mehreren Standards die der Anbieter angegeben hat. Manche äquivalente Standards können strikter sein oder außerhalb der Bedingungen des ursprünglichen Standards.

    Ashby charts

    See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

    Eigenschaften

    Allgemein

    PropertyTemperatureValue

    Dichte

    23.0 °C

    7.8 g/cm³

    Show Material materials with Dichte of 7.8 g/cm³

    Mechanisch

    PropertyTemperatureValueComment

    Dehnung

    23.0 °C

    25 %

    Show Material materials with Dehnung of 25 %

    Elastizitätsmodul

    23.0 °C

    199 GPa

    Show Material materials with Elastizitätsmodul of 199 GPa

    Härte, Brinell

    23.0 °C

    270 [-]

    Show Material materials with Härte, Brinell of 270 [-]

    max.

    Poissonzahl

    23.0 °C

    0.32 [-]

    Show Material materials with Poissonzahl of 0.32 [-]

    Schubmodule

    23.0 °C

    75 GPa

    Show Material materials with Schubmodule of 75 GPa

    Streckgrenze Rp 0,2

    23.0 °C

    550 MPa

    Show Material materials with Streckgrenze Rp 0,2 of 550 MPa

    Zugfestigkeit

    23.0 °C

    750 MPa

    Show Material materials with Zugfestigkeit of 750 MPa

    Thermisch

    PropertyTemperatureValueComment

    Koeffizient der thermischen Ausdehnung

    23.0 °C

    1.11E-5 1/K

    Show Material materials with Koeffizient der thermischen Ausdehnung of 1.11E-5 1/K

    for 20-100°C

    Spezifische Wärmekapazität

    23.0 °C

    425 J/(kg·K)

    Show Material materials with Spezifische Wärmekapazität of 425 J/(kg·K)

    Wärmeleitfähigkeit

    23.0 °C

    14 W/(m·K)

    Show Material materials with Wärmeleitfähigkeit of 14 W/(m·K)

    for 20-300°C

    Elektrisch

    PropertyTemperatureValue

    spezifischer Widerstand

    23.0 °C

    8E-7 Ω·m

    Show Material materials with spezifischer Widerstand of 8E-7 Ω·m

    Magnetisch

    PropertyTemperatureValue

    Relative magnetische Permeabilität

    23.0 °C

    33 [-]

    Show Material materials with Relative magnetische Permeabilität of 33 [-]

    Chemical properties

    PropertyValueComment

    Chrom

    24 - 26 %

    Show Material materials with Chrom of 24 - 26 %

    Eisen

    Balance

    Kohlenstoff

    0.03 %

    Show Material materials with Kohlenstoff of 0.03 %

    max.

    Kupfer

    0.5 - 1 %

    Show Material materials with Kupfer of 0.5 - 1 %

    Mangan

    1 %

    Show Material materials with Mangan of 1 %

    max.

    Molybdän

    3 - 4 %

    Show Material materials with Molybdän of 3 - 4 %

    Nickel

    6 - 8 %

    Show Material materials with Nickel of 6 - 8 %

    Phosphor

    0.03 %

    Show Material materials with Phosphor of 0.03 %

    max.

    Schwefel

    0.01 %

    Show Material materials with Schwefel of 0.01 %

    max.

    Silizium

    1 %

    Show Material materials with Silizium of 1 %

    max.

    Stickstoff

    0.2 - 0.3 %

    Show Material materials with Stickstoff of 0.2 - 0.3 %

    Wolfram

    0.5 - 1 %

    Show Material materials with Wolfram of 0.5 - 1 %

    Technological properties

    Property
    Application areas

    Offshore & marine: Offshore platforms, components for gas, oil and process cooling plants, instrumentation, wellhead and subsea wellhead fittings, desalination plants, seawater cooled heat exchangers, cargo heating systems, marine shafts (for boats etc) and high strength fasteners;Chemical processing: Equipment handling organic or dilute sulphuric acid, process solutions contaminated with chlorides, refinery equipment, desulphurising and distillation units, sewage plant components, fire extinguishing systems, general processing and mixing plant

    Corrosion properties