Mechanisch
Property | Value | Comment |
---|---|---|
Härte, Brinell | 220 [-] Show Supplier Material materials with Härte, Brinell of 220 [-] | soft annealed |
Härte, Rockwell C | 54 - 58 [-] Show Supplier Material materials with Härte, Rockwell C of 54 - 58 [-] | |
Zugfestigkeit | 1665 - 2180 MPa Show Supplier Material materials with Zugfestigkeit of 1665 - 2180 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 200 °C | 1.22e-05 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.22e-05 1/K | for 20°C to the mentioned temperature |
400 °C | 1.25e-05 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.25e-05 1/K | for 20°C to the mentioned temperature | |
Wärmeleitfähigkeit | 100 °C | 28.9 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 28.9 W/(m·K) | |
200 °C | 30 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 30 W/(m·K) | ||
400 °C | 31 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 31 W/(m·K) |
Chemical properties
Property | Value |
---|---|
Chrom | 3.35 % Show Supplier Material materials with Chrom of 3.35 % |
Eisen | Balance |
Kohlenstoff | 0.5 % Show Supplier Material materials with Kohlenstoff of 0.5 % |
Mangan | 0.7 % Show Supplier Material materials with Mangan of 0.7 % |
Molybdän | 1.6 % Show Supplier Material materials with Molybdän of 1.6 % |
Silizium | 0.3 % Show Supplier Material materials with Silizium of 0.3 % |
Vanadium | 0.25 % Show Supplier Material materials with Vanadium of 0.25 % |
Technological properties
Property | ||
---|---|---|
Application areas | Punching tools, moulds, scrap shears, piercing dies, hobs, coining dies, plastic moulds, tableting tools | |
Heat Treatment | Soft annealing: 610-650°C (Cooling in furnace) - Stress-relief-annealing: 600°C, Hardening: 920-970°C and quenching in oil or air |