Allgemein
Property | Value |
---|---|
Partikelgrößenbereich | 20 - 53 µm Show Supplier Material materials with Partikelgrößenbereich of 20 - 53 µm |
Schüttdichte | 3.8 - 4.6 g/cm³ Show Supplier Material materials with Schüttdichte of 3.8 - 4.6 g/cm³ |
Mechanisch
Property | Value | Comment |
---|---|---|
Dehnung | 65 % Show Supplier Material materials with Dehnung of 65 % | A5 |
Härte, Rockwell C | 37 [-] Show Supplier Material materials with Härte, Rockwell C of 37 [-] | |
Streckgrenze | 900 - 950 MPa Show Supplier Material materials with Streckgrenze of 900 - 950 MPa | RP02 |
Zugfestigkeit | 980 - 1080 MPa Show Supplier Material materials with Zugfestigkeit of 980 - 1080 MPa |
Rheological Properties
Property | Value |
---|---|
Halldurchfluss | 12 - 20 s/50g Show Supplier Material materials with Halldurchfluss of 12 - 20 s/50g |
Chemical properties
Property | Value |
---|---|
Eisen | Balance |
Kobalt | 13.5 % Show Supplier Material materials with Kobalt of 13.5 % |
Kohlenstoff | 0.02 % Show Supplier Material materials with Kohlenstoff of 0.02 % |
Mangan | 0.5 % Show Supplier Material materials with Mangan of 0.5 % |
Molybdän | 5 % Show Supplier Material materials with Molybdän of 5 % |
Nickel | 18 % Show Supplier Material materials with Nickel of 18 % |
Silizium | 0.5 % Show Supplier Material materials with Silizium of 0.5 % |
Technological properties
Property | ||
---|---|---|
Application areas | Additive Manufacturing | |
Heat Treatment | Solution annealed (vacuum, 850°C/ 1h/ gas quenching) and ageing (480°C, 4h, air cooling) | |
Processing history | The powder is produced by gas atomization. | |
Processing methods | Der Printdur® Powderfort can be processed on LPBF systems. The process parameters are similar to those of 1.2709. Please contact us for further information. |