Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 2.4 - 2.5 g/cm³ Show Material materials with Dichte of 2.4 - 2.5 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Elastizitätsmodul | 23.0 °C | 70 - 80 GPa Show Material materials with Elastizitätsmodul of 70 - 80 GPa |
Härte, Vickers | 23.0 °C | 480 - 670 [-] Show Material materials with Härte, Vickers of 480 - 670 [-] |
Poissonzahl | 23.0 °C | 0.2 [-] Show Material materials with Poissonzahl of 0.2 [-] |
Schubmodule | 23.0 °C | 26 - 31.7 GPa Show Material materials with Schubmodule of 26 - 31.7 GPa |
Thermisch
Property | Temperature | Value |
---|---|---|
Glühtemperatur | 610 - 650 °C Show Material materials with Glühtemperatur of 610 - 650 °C | |
Koeffizient der thermischen Ausdehnung | 300.0 °C | 3.38E-6 - 9.8E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 3.38E-6 - 9.8E-6 1/K |
Vicat-Erweichungstemperatur | 820 - 910 °C Show Material materials with Vicat-Erweichungstemperatur of 820 - 910 °C |
Optisch
Property | Value |
---|---|
Brechungsindex | 1.49 - 1.51 [-] Show Material materials with Brechungsindex of 1.49 - 1.51 [-] |