Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 8.02 g/cm³ Show Material materials with Dichte of 8.02 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Elastizitätsmodul | 23.0 °C | 195 GPa Show Material materials with Elastizitätsmodul of 195 GPa | Typical for Austenitic Stainless Steel |
Flächenreduzierung | 20.0 °C | 51 % Show Material materials with Flächenreduzierung of 51 % | |
650.0 °C | 41 % Show Material materials with Flächenreduzierung of 41 % | ||
760.0 °C | 50 % Show Material materials with Flächenreduzierung of 50 % | ||
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Austenitic Stainless Steel |
Schubmodule | 23.0 °C | 77 GPa Show Material materials with Schubmodule of 77 GPa | Typical for Austenitic Stainless Steel |
Streckgrenze | 20.0 °C | 470 MPa Show Material materials with Streckgrenze of 470 MPa | |
650.0 °C | 230 MPa Show Material materials with Streckgrenze of 230 MPa | ||
760.0 °C | 170 MPa Show Material materials with Streckgrenze of 170 MPa | ||
Zugfestigkeit | 20.0 °C | 880 MPa Show Material materials with Zugfestigkeit of 880 MPa | |
650.0 °C | 52 MPa Show Material materials with Zugfestigkeit of 52 MPa | ||
760.0 °C | 320 MPa Show Material materials with Zugfestigkeit of 320 MPa | ||
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 760.0 °C | 1.93E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.93E-5 1/K | The mentioned value is between 20°C and the mentioned temperature |
Schmelzpunkt | 1230 - 1480 °C Show Material materials with Schmelzpunkt of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Spezifische Wärmekapazität | 23.0 °C | 440 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 440 J/(kg·K) | Typical for Austenitic Stainless Steel |
Wärmeleitfähigkeit | 23.0 °C | 11 - 21 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 11 - 21 W/(m·K) | Typical for Austenitic Stainless Steel |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
spezifischer Widerstand | 23.0 °C | 8.5E-7 Ω·m Show Material materials with spezifischer Widerstand of 8.5E-7 Ω·m | Typical for Austenitic Stainless Steel |
Chemical properties
Property | Value | Comment |
---|---|---|
Chrom | 12 - 15 % Show Material materials with Chrom of 12 - 15 % | |
Eisen | 64.2 - 73.65 % Show Material materials with Eisen of 64.2 - 73.65 % | Balance |
Kohlenstoff | 0.35 - 0.5 % Show Material materials with Kohlenstoff of 0.35 - 0.5 % | |
Mangan | 1 % Show Material materials with Mangan of 1 % | |
Molybdän | 0.2 - 0.5 % Show Material materials with Molybdän of 0.2 - 0.5 % | |
Nickel | 12 - 15 % Show Material materials with Nickel of 12 - 15 % | |
Phosphor | 0.05 % Show Material materials with Phosphor of 0.05 % | |
Schwefel | 0.03 % Show Material materials with Schwefel of 0.03 % | |
Silizium | 0.3 - 0.8 % Show Material materials with Silizium of 0.3 - 0.8 % | |
Wolfram | 1.5 - 3 % Show Material materials with Wolfram of 1.5 - 3 % |