Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 8.47 g/cm³ Show Material materials with Dichte of 8.47 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Elastizitätsmodul | 23.0 °C | 190 - 210 GPa Show Material materials with Elastizitätsmodul of 190 - 210 GPa | Typical for Steel |
Flächenreduzierung | 20.0 °C | 18 % Show Material materials with Flächenreduzierung of 18 % | |
650.0 °C | 29 % Show Material materials with Flächenreduzierung of 29 % | ||
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Steel |
Streckgrenze | 20.0 °C | 1330 MPa Show Material materials with Streckgrenze of 1330 MPa | |
650.0 °C | 470 MPa Show Material materials with Streckgrenze of 470 MPa | ||
Zugfestigkeit | 20.0 °C | 1570 MPa Show Material materials with Zugfestigkeit of 1570 MPa | |
650.0 °C | 572 MPa Show Material materials with Zugfestigkeit of 572 MPa | ||
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 760.0 °C | 1.4E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4E-5 1/K | The mentioned value is between 20°C and the mentioned temperature |
Chemical properties
Property | Value |
---|---|
Chrom | 3.5 % Show Material materials with Chrom of 3.5 % |
Eisen | 81.55 - 100 % Show Material materials with Eisen of 81.55 - 100 % |
Kohlenstoff | 0.55 % Show Material materials with Kohlenstoff of 0.55 % |
Mangan | 0.2 % Show Material materials with Mangan of 0.2 % |
Silizium | 0.2 % Show Material materials with Silizium of 0.2 % |
Wolfram | 14 % Show Material materials with Wolfram of 14 % |