Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 20.0 °C | 7.8 - 7.9 g/cm³ Show Material materials with Dichte of 7.8 - 7.9 g/cm³ | Typical for Chromium Molybdenum Steel |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung A5 | 20.0 °C | 18 % Show Material materials with Dehnung A5 of 18 % | |
Elastizitätsmodul | 20.0 °C | 200 - 215 GPa Show Material materials with Elastizitätsmodul of 200 - 215 GPa | Typical for Chromium Molybdenum Steel |
Flächenreduzierung | 20.0 °C | 58 % Show Material materials with Flächenreduzierung of 58 % | |
Härte, Rockwell C | 20.0 °C | 35 [-] Show Material materials with Härte, Rockwell C of 35 [-] | |
Poissonzahl | 20.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Chromium Molybdenum Steel |
Streckgrenze | 20.0 °C | 1000 MPa Show Material materials with Streckgrenze of 1000 MPa | |
Zugfestigkeit | 20.0 °C | 1100 MPa Show Material materials with Zugfestigkeit of 1100 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20.0 °C | 1.1E-5 - 1.4E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.1E-5 - 1.4E-5 1/K | Typical for Chromium Molybdenum Steel |
200.0 °C | 1.1E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.1E-5 1/K | Typical for Chromium Molybdenum Steel | |
300.0 °C | 1.17E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.17E-5 1/K | Typical for Chromium Molybdenum Steel | |
500.0 °C | 1.23E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.23E-5 1/K | Typical for Chromium Molybdenum Steel | |
600.0 °C | 1.26E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.26E-5 1/K | Typical for Chromium Molybdenum Steel | |
Schmelzpunkt | 1382 - 1529 °C Show Material materials with Schmelzpunkt of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Spezifische Wärmekapazität | 20.0 °C | 448 - 502 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 448 - 502 J/(kg·K) | Typical for Chromium Molybdenum Steel |
Wärmeleitfähigkeit | 20.0 °C | 36 - 43 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36 - 43 W/(m·K) | Typical for Chromium Molybdenum Steel |
Chemical properties
Property | Value |
---|---|
Chrom | 0.75 - 1.2 % Show Material materials with Chrom of 0.75 - 1.2 % |
Eisen | Balance |
Kohlenstoff | 0.37 - 0.44 % Show Material materials with Kohlenstoff of 0.37 - 0.44 % |
Mangan | 0.75 - 1.1 % Show Material materials with Mangan of 0.75 - 1.1 % |
Molybdän | 0.15 - 0.25 % Show Material materials with Molybdän of 0.15 - 0.25 % |
Phosphor | 0.35 % Show Material materials with Phosphor of 0.35 % |
Schwefel | 0.04 % Show Material materials with Schwefel of 0.04 % |
Silizium | 0.15 - 0.35 % Show Material materials with Silizium of 0.15 - 0.35 % |