Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 7.8 - 7.9 g/cm³ Show Material materials with Dichte of 7.8 - 7.9 g/cm³ | Typical for Medium Carbon Steel |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 10.2 % Show Material materials with Dehnung of 10.2 % | Predicted Value, A200 | ||||
10.5 % Show Material materials with Dehnung of 10.5 % | Predicted Value, A80 | |||||
10.7 % Show Material materials with Dehnung of 10.7 % | Predicted Value, Transverse | |||||
13.1 % Show Material materials with Dehnung of 13.1 % | Predicted Value, A50 | |||||
16.4 % Show Material materials with Dehnung of 16.4 % | Predicted Value, A5 | |||||
19.1 % Show Material materials with Dehnung of 19.1 % | Predicted Value, A80 Transverse | |||||
20 °C | 13 % Show Material materials with Dehnung of 13 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
Elastizitätsmodul | 200 - 215 GPa Show Material materials with Elastizitätsmodul of 200 - 215 GPa | Typical for Medium Carbon Steel | ||||
Flächenreduzierung | 42.5 % Show Material materials with Flächenreduzierung of 42.5 % | Predicted Value, Transverse | ||||
20 °C | 50 % Show Material materials with Flächenreduzierung of 50 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
Härte, Brinell | 254 [-] Show Material materials with Härte, Brinell of 254 [-] | Predicted Value, Transverse | ||||
Poissonzahl | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Medium Carbon Steel | ||||
Scherfestigkeit | 502.4 MPa Show Material materials with Scherfestigkeit of 502.4 MPa | Predicted Value | ||||
Schubmodule | 75 - 80 GPa Show Material materials with Schubmodule of 75 - 80 GPa | Typical for Carbon Steel | ||||
Streckgrenze | 314 MPa Show Material materials with Streckgrenze of 314 MPa | Predicted Value, RP05 | ||||
320.1 MPa Show Material materials with Streckgrenze of 320.1 MPa | Predicted Value, RP1 | |||||
325.6 MPa Show Material materials with Streckgrenze of 325.6 MPa | Predicted Value, RP1 Transverse | |||||
491.8 MPa Show Material materials with Streckgrenze of 491.8 MPa | Predicted Value, Transverse | |||||
502.3 MPa Show Material materials with Streckgrenze of 502.3 MPa | Predicted Value, RP02 Transverse | |||||
725.9 MPa Show Material materials with Streckgrenze of 725.9 MPa | Predicted Value, RP002 | |||||
762.5 MPa Show Material materials with Streckgrenze of 762.5 MPa | Predicted Value, RP02 | |||||
20 °C | 650 MPa Show Material materials with Streckgrenze of 650 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 800 MPa Show Material materials with Streckgrenze of 800 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
Zugfestigkeit | 20 °C | 800 - 1150 MPa Show Material materials with Zugfestigkeit of 800 - 1150 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | |
20 °C | 800 - 950 MPa Show Material materials with Zugfestigkeit of 800 - 950 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 950 - 1150 MPa Show Material materials with Zugfestigkeit of 950 - 1150 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat | ||
20 °C | 950 MPa Show Material materials with Zugfestigkeit of 950 MPa | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 1.32e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 1/K | Typical for Medium Carbon Steel |
Max. Betriebstemperatur | 305.9 °C Show Material materials with Max. Betriebstemperatur of 305.9 °C | Predicted Value, Long |
500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | Typical for Carbon Steel | |
Schmelzpunkt | 1380 - 1514 °C Show Material materials with Schmelzpunkt of 1380 - 1514 °C | Typical for Medium Carbon Steel |
Spezifische Wärmekapazität | 470 - 520 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 470 - 520 J/(kg·K) | Typical for Medium Carbon Steel |
Wärmeleitfähigkeit | 21 - 52 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 21 - 52 W/(m·K) | Typical for Medium Carbon Steel |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 7 S/m Show Material materials with Elektrische Leitfähigkeit of 7 S/m | Predicted Value |
spezifischer Widerstand | 1.43e-07 - 1.74e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.43e-07 - 1.74e-07 Ω·m | Typical for Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Bor | 0.0008 - 0.005 % Show Material materials with Bor of 0.0008 - 0.005 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |
0.001 - 0.005 % Show Material materials with Bor of 0.001 - 0.005 % | quenched and tempered (+QT) | EN 10083-3, ISO 683-2 | Bar, Forging, Sheet, Strip, Flat | |
Kohlenstoff | 0.27 - 0.33 % Show Material materials with Kohlenstoff of 0.27 - 0.33 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |
Kupfer | 0.4 % Show Material materials with Kupfer of 0.4 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |
Mangan | 1.15 - 1.45 % Show Material materials with Mangan of 1.15 - 1.45 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |
Phosphor | 0.025 % Show Material materials with Phosphor of 0.025 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |
Schwefel | 0.035 % Show Material materials with Schwefel of 0.035 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | quenched and tempered (+QT) | ISO 683-2, EN 10083-3 | Bar, Forging, Sheet, Strip, Flat |