Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 7.7 g/cm³ Show Material materials with Dichte of 7.7 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 40 % Show Material materials with Dehnung of 40 % | |
Dehnung A80, transversal | 20.0 °C | 40 % Show Material materials with Dehnung A80, transversal of 40 % | |
Dehnung, transversal | 20.0 °C | 30 - 40 % Show Material materials with Dehnung, transversal of 30 - 40 % | |
Elastizitätsmodul | 20.0 °C | 200 GPa Show Material materials with Elastizitätsmodul of 200 GPa | |
100.0 °C | 194 GPa Show Material materials with Elastizitätsmodul of 194 GPa | ||
200.0 °C | 186 GPa Show Material materials with Elastizitätsmodul of 186 GPa | ||
300.0 °C | 179 GPa Show Material materials with Elastizitätsmodul of 179 GPa | ||
400.0 °C | 172 GPa Show Material materials with Elastizitätsmodul of 172 GPa | ||
500.0 °C | 165 GPa Show Material materials with Elastizitätsmodul of 165 GPa | ||
Hardness, Brinell, trans | 20.0 °C | 230 [-] Show Material materials with Hardness, Brinell, trans of 230 [-] | |
Härte, Brinell | 20.0 °C | 230 [-] Show Material materials with Härte, Brinell of 230 [-] | |
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Austenitic Stainless Steel |
Schubmodule | 23.0 °C | 77 GPa Show Material materials with Schubmodule of 77 GPa | Typical for Austenitic Stainless Steel |
Streckgrenze Rp 0,2 | 20.0 °C | 210 MPa Show Material materials with Streckgrenze Rp 0,2 of 210 MPa | |
100.0 °C | 185 MPa Show Material materials with Streckgrenze Rp 0,2 of 185 MPa | ||
150.0 °C | 160 MPa Show Material materials with Streckgrenze Rp 0,2 of 160 MPa | ||
200.0 °C | 145 MPa Show Material materials with Streckgrenze Rp 0,2 of 145 MPa | ||
250.0 °C | 135 MPa Show Material materials with Streckgrenze Rp 0,2 of 135 MPa | ||
300.0 °C | 125 MPa Show Material materials with Streckgrenze Rp 0,2 of 125 MPa | ||
350.0 °C | 120 MPa Show Material materials with Streckgrenze Rp 0,2 of 120 MPa | ||
400.0 °C | 115 MPa Show Material materials with Streckgrenze Rp 0,2 of 115 MPa | ||
Streckgrenze Rp 0,2, transversal | 20.0 °C | 210 - 220 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 210 - 220 MPa | |
Streckgrenze Rp 1,0 | 20.0 °C | 240 MPa Show Material materials with Streckgrenze Rp 1,0 of 240 MPa | |
100.0 °C | 210 MPa Show Material materials with Streckgrenze Rp 1,0 of 210 MPa | ||
150.0 °C | 190 MPa Show Material materials with Streckgrenze Rp 1,0 of 190 MPa | ||
200.0 °C | 175 MPa Show Material materials with Streckgrenze Rp 1,0 of 175 MPa | ||
250.0 °C | 165 MPa Show Material materials with Streckgrenze Rp 1,0 of 165 MPa | ||
300.0 °C | 155 MPa Show Material materials with Streckgrenze Rp 1,0 of 155 MPa | ||
350.0 °C | 150 MPa Show Material materials with Streckgrenze Rp 1,0 of 150 MPa | ||
Streckgrenze Rp 1,0, transversal | 20.0 °C | 240 - 260 MPa Show Material materials with Streckgrenze Rp 1,0, transversal of 240 - 260 MPa | |
Zugfestigkeit | 20.0 °C | 530 - 730 MPa Show Material materials with Zugfestigkeit of 530 - 730 MPa | |
Zugfestigkeit, transversal | 20.0 °C | 530 - 730 MPa Show Material materials with Zugfestigkeit, transversal of 530 - 730 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.65E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.65E-5 1/K | |
Schmelzpunkt | 1230 - 1480 °C Show Material materials with Schmelzpunkt of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Spezifische Wärmekapazität | 23.0 °C | 440 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 440 J/(kg·K) | Typical for Austenitic Stainless Steel |
Wärmeleitfähigkeit | 20.0 °C | 14 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 14 W/(m·K) |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
spezifischer Widerstand | 23.0 °C | 8.5E-7 Ω·m Show Material materials with spezifischer Widerstand of 8.5E-7 Ω·m | Typical for Austenitic Stainless Steel |
Chemical properties
Property | Value |
---|---|
Chrom | 16.5 - 18.5 % Show Material materials with Chrom of 16.5 - 18.5 % |
Kohlenstoff | 0.015 % Show Material materials with Kohlenstoff of 0.015 % |
Mangan | 2 % Show Material materials with Mangan of 2 % |
Molybdän | 0.2 % Show Material materials with Molybdän of 0.2 % |
Nickel | 14 - 16 % Show Material materials with Nickel of 14 - 16 % |
Phosphor | 0.03 % Show Material materials with Phosphor of 0.03 % |
Schwefel | 0.01 % Show Material materials with Schwefel of 0.01 % |
Silizium | 3.7 - 4.5 % Show Material materials with Silizium of 3.7 - 4.5 % |
Stickstoff | 0.11 % Show Material materials with Stickstoff of 0.11 % |