Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.85 g/cm³ Show Material materials with Dichte of 7.85 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat |
20 °C | 7.85 - 7.851 g/cm³ Show Material materials with Dichte of 7.85 - 7.851 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
20 °C | 7.851 g/cm³ Show Material materials with Dichte of 7.851 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
50 °C | 7.842 g/cm³ Show Material materials with Dichte of 7.842 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
100 °C | 7.827 g/cm³ Show Material materials with Dichte of 7.827 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
150 °C | 7.811 g/cm³ Show Material materials with Dichte of 7.811 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
200 °C | 7.794 g/cm³ Show Material materials with Dichte of 7.794 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
250 °C | 7.777 g/cm³ Show Material materials with Dichte of 7.777 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
300 °C | 7.76 g/cm³ Show Material materials with Dichte of 7.76 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
350 °C | 7.742 g/cm³ Show Material materials with Dichte of 7.742 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
400 °C | 7.724 g/cm³ Show Material materials with Dichte of 7.724 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 15.5 % Show Material materials with Dehnung of 15.5 % | Predicted Value, A80 Transverse | ||||
15.7 % Show Material materials with Dehnung of 15.7 % | Predicted Value, A200 | |||||
16.6 % Show Material materials with Dehnung of 16.6 % | Predicted Value, A80 | |||||
19.4 % Show Material materials with Dehnung of 19.4 % | Predicted Value, A5 | |||||
20.8 % Show Material materials with Dehnung of 20.8 % | Predicted Value, A50 | |||||
20 °C | 16 % Show Material materials with Dehnung of 16 % | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | Transverse | |
20 °C | 16 % Show Material materials with Dehnung of 16 % | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Elastizitätsmodul | -100 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | |
20 °C | 208.4 - 211 GPa Show Material materials with Elastizitätsmodul of 208.4 - 211 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 208.4 - 212 GPa Show Material materials with Elastizitätsmodul of 208.4 - 212 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 208.4 GPa Show Material materials with Elastizitätsmodul of 208.4 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 211 GPa Show Material materials with Elastizitätsmodul of 211 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 211 - 212 GPa Show Material materials with Elastizitätsmodul of 211 - 212 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
50 °C | 206.9 GPa Show Material materials with Elastizitätsmodul of 206.9 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 204.1 - 206 GPa Show Material materials with Elastizitätsmodul of 204.1 - 206 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 204.1 - 207 GPa Show Material materials with Elastizitätsmodul of 204.1 - 207 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 204.1 GPa Show Material materials with Elastizitätsmodul of 204.1 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 206 GPa Show Material materials with Elastizitätsmodul of 206 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 206 - 207 GPa Show Material materials with Elastizitätsmodul of 206 - 207 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
150 °C | 200.6 GPa Show Material materials with Elastizitätsmodul of 200.6 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 196.9 - 200 GPa Show Material materials with Elastizitätsmodul of 196.9 - 200 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 196.9 - 199 GPa Show Material materials with Elastizitätsmodul of 196.9 - 199 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 196.9 GPa Show Material materials with Elastizitätsmodul of 196.9 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 199 - 200 GPa Show Material materials with Elastizitätsmodul of 199 - 200 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
200 °C | 200 GPa Show Material materials with Elastizitätsmodul of 200 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
250 °C | 193.2 GPa Show Material materials with Elastizitätsmodul of 193.2 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 189.2 - 192 GPa Show Material materials with Elastizitätsmodul of 189.2 - 192 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 189.2 GPa Show Material materials with Elastizitätsmodul of 189.2 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
350 °C | 185.2 GPa Show Material materials with Elastizitätsmodul of 185.2 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 181.0 - 184 GPa Show Material materials with Elastizitätsmodul of 181.0 - 184 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 181.0 GPa Show Material materials with Elastizitätsmodul of 181.0 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
500 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 164 GPa Show Material materials with Elastizitätsmodul of 164 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Flächenreduzierung | 39.2 % Show Material materials with Flächenreduzierung of 39.2 % | Predicted Value | ||||
44.4 % Show Material materials with Flächenreduzierung of 44.4 % | Predicted Value, Transverse | |||||
Härte, Brinell | 253 [-] Show Material materials with Härte, Brinell of 253 [-] | Predicted Value, Transverse | ||||
Poissonzahl | 20 °C | 0.289 [-] Show Material materials with Poissonzahl of 0.289 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | |
50 °C | 0.289 [-] Show Material materials with Poissonzahl of 0.289 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 0.291 [-] Show Material materials with Poissonzahl of 0.291 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
150 °C | 0.291 [-] Show Material materials with Poissonzahl of 0.291 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 0.292 [-] Show Material materials with Poissonzahl of 0.292 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
250 °C | 0.294 [-] Show Material materials with Poissonzahl of 0.294 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 0.295 [-] Show Material materials with Poissonzahl of 0.295 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
350 °C | 0.298 [-] Show Material materials with Poissonzahl of 0.298 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 0.305 [-] Show Material materials with Poissonzahl of 0.305 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Scherfestigkeit | 637.1 MPa Show Material materials with Scherfestigkeit of 637.1 MPa | Predicted Value | ||||
Schubmodule | 20 °C | 80.8 GPa Show Material materials with Schubmodule of 80.8 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | |
50 °C | 80.2 GPa Show Material materials with Schubmodule of 80.2 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 79.0 GPa Show Material materials with Schubmodule of 79.0 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
150 °C | 77.7 GPa Show Material materials with Schubmodule of 77.7 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 76.2 GPa Show Material materials with Schubmodule of 76.2 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
250 °C | 74.7 GPa Show Material materials with Schubmodule of 74.7 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 73.1 GPa Show Material materials with Schubmodule of 73.1 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
350 °C | 71.3 GPa Show Material materials with Schubmodule of 71.3 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 69.4 GPa Show Material materials with Schubmodule of 69.4 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Zugfestigkeit | 20 °C | 580 - 740 MPa Show Material materials with Zugfestigkeit of 580 - 740 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | Transverse |
20 °C | 580 - 740 MPa Show Material materials with Zugfestigkeit of 580 - 740 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 590 - 740 MPa Show Material materials with Zugfestigkeit of 590 - 740 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.05e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | |
20 °C | 1.15e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.15e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
100 °C | 1.21e-05 - 1.22e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 - 1.22e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 1.21e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
100 °C | 1.22e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.22e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 1.27e-05 - 1.29e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27e-05 - 1.29e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 1.27e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
200 °C | 1.29e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.29e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 1.32e-05 - 1.34e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 - 1.34e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 1.32e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
300 °C | 1.34e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.34e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 1.36e-05 - 1.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 - 1.4e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
400 °C | 1.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 1.43e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.43e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 1.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.46e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Max. Betriebstemperatur | -10 - 500 °C Show Material materials with Max. Betriebstemperatur of -10 - 500 °C | quenched and tempered (+QT) | EN 10028-2 | Flat | Long | |
20 - 500 °C Show Material materials with Max. Betriebstemperatur of 20 - 500 °C | quenched and tempered (+QT) | EN 10028-2 | Flat | Long | ||
Spezifische Wärmekapazität | -100 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | |
20 °C | 430 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 430 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 430 - 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 430 - 461 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
100 °C | 479 - 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 - 500 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
100 °C | 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 500 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 499 - 540 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 - 540 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
200 °C | 540 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 540 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 517 - 580 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 - 580 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
300 °C | 580 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 580 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 536 - 620 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 - 620 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
400 °C | 620 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 620 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 690 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 690 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 780 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 780 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Temperaturleitfähigkeit | 20 °C | 10.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 10.7 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | |
100 °C | 10.4 mm²/s Show Material materials with Temperaturleitfähigkeit of 10.4 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
200 °C | 9.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.9 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
300 °C | 9.2 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.2 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
400 °C | 8.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.3 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
Wärmeleitfähigkeit | 20 °C | 38 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | |
20 °C | 38 - 38.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38 - 38.6 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 38.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38.6 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
100 °C | 40.4 - 41 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 40.4 - 41 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 40.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 40.4 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
100 °C | 41 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 41 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 41.3 - 42 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 41.3 - 42 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 41.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 41.3 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
200 °C | 42 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 40.7 - 41 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 40.7 - 41 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 40.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 40.7 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
300 °C | 41 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 41 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 39 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 39 - 39.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39 - 39.3 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 39.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39.3 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
500 °C | 38 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 35 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 35 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 5 S/m Show Material materials with Elektrische Leitfähigkeit of 5 S/m | Predicted Value | ||||
spezifischer Widerstand | 20 °C | 2.7e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.7e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | |
50 °C | 2.87e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.87e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 3.17e-07 - 3.2e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.17e-07 - 3.2e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 3.17e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.17e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
100 °C | 3.2e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.2e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
150 °C | 3.49e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.49e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 3.8e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.8e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 3.8e-07 - 3.82e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.8e-07 - 3.82e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 3.82e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.82e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
250 °C | 4.21e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.21e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 4.6e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.6e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 4.6e-07 - 4.61e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.6e-07 - 4.61e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 4.61e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.61e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
350 °C | 5.06e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.06e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 5.5e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.5e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 5.5e-07 - 5.54e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.5e-07 - 5.54e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 5.54e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.54e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet | ||
500 °C | 6.6e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.6e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 7.8e-07 Ω·m Show Material materials with spezifischer Widerstand of 7.8e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.015 % Show Material materials with Aluminium of 0.015 % | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet |
Chrom | 0.3 % Show Material materials with Chrom of 0.3 % | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet |
Kohlenstoff | 0.17 % Show Material materials with Kohlenstoff of 0.17 % | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet |
Kupfer | 0.5 - 0.8 % Show Material materials with Kupfer of 0.5 - 0.8 % | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet |
Mangan | 0.8 - 1.2 % Show Material materials with Mangan of 0.8 - 1.2 % | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet |
Molybdän | 0.25 - 0.5 % Show Material materials with Molybdän of 0.25 - 0.5 % | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet |
Nickel | 1 - 1.3 % Show Material materials with Nickel of 1 - 1.3 % | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet |
Niobium | 0.015 - 0.045 % Show Material materials with Niobium of 0.015 - 0.045 % | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet |
Phosphor | 0.03 % Show Material materials with Phosphor of 0.03 % | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet |
Schwefel | 0.01 % Show Material materials with Schwefel of 0.01 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
0.025 % Show Material materials with Schwefel of 0.025 % | quenched and tempered (+QT) | EN 10028-2 | Sheet, Flat | |
Silizium | 0.25 - 0.5 % Show Material materials with Silizium of 0.25 - 0.5 % | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet |
Stickstoff | 0.02 % Show Material materials with Stickstoff of 0.02 % | quenched and tempered (+QT) | EN 10028-2 | Flat, Sheet |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |