Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.46 g/cm³ Show Material materials with Dichte of 8.46 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | -80.0 °C | 18 % Show Material materials with Dehnung of 18 % |
20.0 °C | 17 - 23 % Show Material materials with Dehnung of 17 - 23 % | |
100.0 °C | 23 % Show Material materials with Dehnung of 23 % | |
200.0 °C | 23 % Show Material materials with Dehnung of 23 % | |
300.0 °C | 23 % Show Material materials with Dehnung of 23 % | |
400.0 °C | 12 % Show Material materials with Dehnung of 12 % | |
500.0 °C | 4.5 % Show Material materials with Dehnung of 4.5 % | |
600.0 °C | 1.5 % Show Material materials with Dehnung of 1.5 % | |
700.0 °C | 3.5 % Show Material materials with Dehnung of 3.5 % | |
Elastizitätsmodul | 20.0 °C | 178.54 GPa Show Material materials with Elastizitätsmodul of 178.54 GPa |
100.0 °C | 174.62 GPa Show Material materials with Elastizitätsmodul of 174.62 GPa | |
200.0 °C | 170.69 GPa Show Material materials with Elastizitätsmodul of 170.69 GPa | |
300.0 °C | 165.79 GPa Show Material materials with Elastizitätsmodul of 165.79 GPa | |
400.0 °C | 159.9 GPa Show Material materials with Elastizitätsmodul of 159.9 GPa | |
500.0 °C | 153.04 GPa Show Material materials with Elastizitätsmodul of 153.04 GPa | |
Härte, Brinell | 20.0 °C | 265 [-] Show Material materials with Härte, Brinell of 265 [-] |
Streckgrenze Rp 0,2 | -80.0 °C | 785 MPa Show Material materials with Streckgrenze Rp 0,2 of 785 MPa |
20.0 °C | 687 - 755 MPa Show Material materials with Streckgrenze Rp 0,2 of 687 - 755 MPa | |
100.0 °C | 736 MPa Show Material materials with Streckgrenze Rp 0,2 of 736 MPa | |
200.0 °C | 716 MPa Show Material materials with Streckgrenze Rp 0,2 of 716 MPa | |
300.0 °C | 716 MPa Show Material materials with Streckgrenze Rp 0,2 of 716 MPa | |
400.0 °C | 716 MPa Show Material materials with Streckgrenze Rp 0,2 of 716 MPa | |
500.0 °C | 677 MPa Show Material materials with Streckgrenze Rp 0,2 of 677 MPa | |
600.0 °C | 579 MPa Show Material materials with Streckgrenze Rp 0,2 of 579 MPa | |
700.0 °C | 441 MPa Show Material materials with Streckgrenze Rp 0,2 of 441 MPa | |
Zugfestigkeit | -80.0 °C | 1177 MPa Show Material materials with Zugfestigkeit of 1177 MPa |
20.0 °C | 962 - 1079 MPa Show Material materials with Zugfestigkeit of 962 - 1079 MPa | |
100.0 °C | 1030 MPa Show Material materials with Zugfestigkeit of 1030 MPa | |
200.0 °C | 1020 MPa Show Material materials with Zugfestigkeit of 1020 MPa | |
300.0 °C | 1010 MPa Show Material materials with Zugfestigkeit of 1010 MPa | |
400.0 °C | 903 MPa Show Material materials with Zugfestigkeit of 903 MPa | |
500.0 °C | 726 MPa Show Material materials with Zugfestigkeit of 726 MPa | |
600.0 °C | 589 MPa Show Material materials with Zugfestigkeit of 589 MPa | |
700.0 °C | 461 MPa Show Material materials with Zugfestigkeit of 461 MPa | |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.4E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4E-5 1/K | |
300.0 °C | 1.5E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.5E-5 1/K | ||
600.0 °C | 1.6E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6E-5 1/K | ||
Max. Betriebstemperatur, lang | 0 - 450 °C Show Material materials with Max. Betriebstemperatur, lang of 0 - 450 °C | ||
Schmelzpunkt | 1170 - 1365 °C Show Material materials with Schmelzpunkt of 1170 - 1365 °C | Typical for Nickel Copper Alloy | |
Spezifische Wärmekapazität | 20.0 °C | 427 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 427 J/(kg·K) | |
100.0 °C | 427 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 427 J/(kg·K) | ||
Wärmeleitfähigkeit | 20.0 °C | 18 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 18 W/(m·K) | |
100.0 °C | 18 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 18 W/(m·K) | ||
Elektrisch
Property | Temperature | Value |
---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 1.72E+6 S/m Show Material materials with Elektrische Leitfähigkeit of 1.72E+6 S/m |
spezifischer Widerstand | 20.0 °C | 5.47E-7 Ω·m Show Material materials with spezifischer Widerstand of 5.47E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Aluminium | 2 - 4 % Show Material materials with Aluminium of 2 - 4 % |
Eisen | 2 % Show Material materials with Eisen of 2 % |
Kobalt | 1 % Show Material materials with Kobalt of 1 % |
Kohlenstoff | 0.25 % Show Material materials with Kohlenstoff of 0.25 % |
Kupfer | 27 - 34 % Show Material materials with Kupfer of 27 - 34 % |
Mangan | 1.5 % Show Material materials with Mangan of 1.5 % |
Schwefel | 0.01 % Show Material materials with Schwefel of 0.01 % |
Silizium | 1 % Show Material materials with Silizium of 1 % |
Titan | 0.25 - 1 % Show Material materials with Titan of 0.25 - 1 % |