Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | T6 | BS 1474 | Bar, Tube, Plate |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Dehnung | 6.0 - 8.0 % Show Material materials with Dehnung of 6.0 - 8.0 % | T6 | BS 1474 | Bar, Tube, Plate | |
Elastizitätsmodul | 70 GPa Show Material materials with Elastizitätsmodul of 70 GPa | T6 | BS 1474 | Bar, Tube, Plate | |
Härte, Brinell | 84.0 - 91.0 [-] Show Material materials with Härte, Brinell of 84.0 - 91.0 [-] | T6 | BS 1474 | Bar, Tube, Plate | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | |||
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | |||
Streckgrenze | 270 MPa Show Material materials with Streckgrenze of 270 MPa | T6 | BS 1474 | Bar, Tube, Plate | |
Zugfestigkeit | 310 MPa Show Material materials with Zugfestigkeit of 310 MPa | T6 | BS 1474 | Bar, Tube, Plate |
Thermisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | T6 | BS 1474 | Bar, Tube, Plate | |
Schmelzpunkt | 555.0 °C Show Material materials with Schmelzpunkt of 555.0 °C | T6 | BS 1474 | Bar, Tube, Plate | |
Spezifische Wärmekapazität | 887.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium | |||
Wärmeleitfähigkeit | 180 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 180 W/(m·K) | T6 | BS 1474 | Bar, Tube, Plate |
Elektrisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 21000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 21000000.0 - 34000000.0 S/m | Typical for Wrought 6000 Series Aluminium | |||
spezifischer Widerstand | 3.7999999999999996e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.7999999999999996e-08 Ω·m | T6 | BS 1474 | Bar, Tube, Plate |
Chemical properties
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Andere | 0.15 Show Material materials with Andere of 0.15 | T6 | BS 1474 | Bar, Tube, Plate | Total |
Chrom | 0.25 Show Material materials with Chrom of 0.25 | T6 | BS 1474 | Bar, Tube, Plate | |
Eisen | 0.5 Show Material materials with Eisen of 0.5 | T6 | BS 1474 | Bar, Tube, Plate | |
Kupfer | 0.1 Show Material materials with Kupfer of 0.1 | T6 | BS 1474 | Bar, Tube, Plate | |
Magnesium | 0.6 - 1.2 % Show Material materials with Magnesium of 0.6 - 1.2 % | T6 | BS 1474 | Bar, Tube, Plate | |
Mangan | 0.4 - 1.0 % Show Material materials with Mangan of 0.4 - 1.0 % | T6 | BS 1474 | Bar, Tube, Plate | |
Silizium | 0.7 - 1.3 % Show Material materials with Silizium of 0.7 - 1.3 % | T6 | BS 1474 | Bar, Tube, Plate | |
Titan | 0.1 Show Material materials with Titan of 0.1 | T6 | BS 1474 | Bar, Tube, Plate | |
Zink | 0.2 Show Material materials with Zink of 0.2 | T6 | BS 1474 | Bar, Tube, Plate |
Technological properties
Property | ||
---|---|---|
Workability | Excellent workability. |