Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.12 g/cm³ Show Material materials with Dichte of 8.12 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Elastizitätsmodul | 20.0 °C | 224 GPa Show Material materials with Elastizitätsmodul of 224 GPa | |
100.0 °C | 220 GPa Show Material materials with Elastizitätsmodul of 220 GPa | ||
200.0 °C | 214 GPa Show Material materials with Elastizitätsmodul of 214 GPa | ||
300.0 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | ||
400.0 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | ||
500.0 °C | 191 GPa Show Material materials with Elastizitätsmodul of 191 GPa | ||
600.0 °C | 180 GPa Show Material materials with Elastizitätsmodul of 180 GPa | ||
Poissonzahl | 20.0 °C | 0.28 [-] Show Material materials with Poissonzahl of 0.28 [-] | |
Schubmodule | 23.0 °C | 79 GPa Show Material materials with Schubmodule of 79 GPa | Typical for Tool And Machining Steel |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100.0 °C | 9.6E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 9.6E-6 1/K | |
20.0 °C | 1.05E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05E-5 1/K | ||
100.0 °C | 1.11E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.11E-5 1/K | ||
200.0 °C | 1.16E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.16E-5 1/K | ||
300.0 °C | 1.2E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.2E-5 1/K | ||
400.0 °C | 1.24E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.24E-5 1/K | ||
500.0 °C | 1.27E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27E-5 1/K | ||
600.0 °C | 1.3E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.3E-5 1/K | ||
Schmelzpunkt | 1370 - 1425 °C Show Material materials with Schmelzpunkt of 1370 - 1425 °C | Typical for Tool And Machining Steel | |
Spezifische Wärmekapazität | 23.0 °C | 420 - 460 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 420 - 460 J/(kg·K) | Typical for Tool And Machining Steel |
Wärmeleitfähigkeit | 20.0 °C | 27.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 27.6 W/(m·K) | |
100.0 °C | 27.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 27.9 W/(m·K) | ||
200.0 °C | 27.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 27.7 W/(m·K) | ||
300.0 °C | 27.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 27.5 W/(m·K) | ||
400.0 °C | 27 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 27 W/(m·K) | ||
500.0 °C | 26.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 26.6 W/(m·K) | ||
600.0 °C | 26.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 26.1 W/(m·K) | ||
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 5.24E-7 Ω·m Show Material materials with spezifischer Widerstand of 5.24E-7 Ω·m |
100.0 °C | 5.81E-7 Ω·m Show Material materials with spezifischer Widerstand of 5.81E-7 Ω·m | |
200.0 °C | 6.64E-7 Ω·m Show Material materials with spezifischer Widerstand of 6.64E-7 Ω·m | |
300.0 °C | 7.51E-7 Ω·m Show Material materials with spezifischer Widerstand of 7.51E-7 Ω·m | |
400.0 °C | 8.44E-7 Ω·m Show Material materials with spezifischer Widerstand of 8.44E-7 Ω·m | |
500.0 °C | 9.41E-7 Ω·m Show Material materials with spezifischer Widerstand of 9.41E-7 Ω·m | |
600.0 °C | 1.04E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.04E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Chrom | 3.8 - 4.5 % Show Material materials with Chrom of 3.8 - 4.5 % |
Kohlenstoff | 0.95 - 1.03 % Show Material materials with Kohlenstoff of 0.95 - 1.03 % |
Mangan | 0.4 % Show Material materials with Mangan of 0.4 % |
Molybdän | 2.5 - 2.9 % Show Material materials with Molybdän of 2.5 - 2.9 % |
Phosphor | 0.03 % Show Material materials with Phosphor of 0.03 % |
Schwefel | 0.45 % Show Material materials with Schwefel of 0.45 % |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % |
Vanadium | 2.2 - 2.5 % Show Material materials with Vanadium of 2.2 - 2.5 % |
Wolfram | 2.7 - 3 % Show Material materials with Wolfram of 2.7 - 3 % |