Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 7.65 - 7.7 g/cm³ Show Material materials with Dichte of 7.65 - 7.7 g/cm³ |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 20 % Show Material materials with Dehnung of 20 % |
Dehnung, transversal | 20.0 °C | 15 - 18 % Show Material materials with Dehnung, transversal of 15 - 18 % |
Elastizitätsmodul | 20.0 °C | 196 - 231.66 GPa Show Material materials with Elastizitätsmodul of 196 - 231.66 GPa |
95.0 °C | 227.53 GPa Show Material materials with Elastizitätsmodul of 227.53 GPa | |
100.0 °C | 218 GPa Show Material materials with Elastizitätsmodul of 218 GPa | |
150.0 °C | 223.39 GPa Show Material materials with Elastizitätsmodul of 223.39 GPa | |
200.0 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | |
205.0 °C | 218.56 GPa Show Material materials with Elastizitätsmodul of 218.56 GPa | |
260.0 °C | 213.74 GPa Show Material materials with Elastizitätsmodul of 213.74 GPa | |
300.0 °C | 205 GPa Show Material materials with Elastizitätsmodul of 205 GPa | |
315.0 °C | 209.6 GPa Show Material materials with Elastizitätsmodul of 209.6 GPa | |
370.0 °C | 204.09 GPa Show Material materials with Elastizitätsmodul of 204.09 GPa | |
400.0 °C | 197 GPa Show Material materials with Elastizitätsmodul of 197 GPa | |
425.0 °C | 198.57 GPa Show Material materials with Elastizitätsmodul of 198.57 GPa | |
485.0 °C | 193.05 GPa Show Material materials with Elastizitätsmodul of 193.05 GPa | |
540.0 °C | 187.54 GPa Show Material materials with Elastizitätsmodul of 187.54 GPa | |
595.0 °C | 180.64 GPa Show Material materials with Elastizitätsmodul of 180.64 GPa | |
650.0 °C | 173.06 GPa Show Material materials with Elastizitätsmodul of 173.06 GPa | |
705.0 °C | 162.72 GPa Show Material materials with Elastizitätsmodul of 162.72 GPa | |
760.0 °C | 151.69 GPa Show Material materials with Elastizitätsmodul of 151.69 GPa | |
815.0 °C | 144.79 GPa Show Material materials with Elastizitätsmodul of 144.79 GPa | |
Hardness, Brinell, trans | 20.0 °C | 185 [-] Show Material materials with Hardness, Brinell, trans of 185 [-] |
Härte, Brinell | 20.0 °C | 185 [-] Show Material materials with Härte, Brinell of 185 [-] |
Härte, Vickers | 20.0 °C | 185 [-] Show Material materials with Härte, Vickers of 185 [-] |
Poissonzahl | 20.0 °C | 0.24 [-] Show Material materials with Poissonzahl of 0.24 [-] |
95.0 °C | 0.27 [-] Show Material materials with Poissonzahl of 0.27 [-] | |
150.0 °C | 0.28 [-] Show Material materials with Poissonzahl of 0.28 [-] | |
205.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
260.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
315.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
370.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
425.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
485.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | |
540.0 °C | 0.31 [-] Show Material materials with Poissonzahl of 0.31 [-] | |
595.0 °C | 0.31 [-] Show Material materials with Poissonzahl of 0.31 [-] | |
650.0 °C | 0.34 [-] Show Material materials with Poissonzahl of 0.34 [-] | |
705.0 °C | 0.34 [-] Show Material materials with Poissonzahl of 0.34 [-] | |
760.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | |
815.0 °C | 0.35 [-] Show Material materials with Poissonzahl of 0.35 [-] | |
Schubmodule | 20.0 °C | 93.08 GPa Show Material materials with Schubmodule of 93.08 GPa |
95.0 °C | 89.63 GPa Show Material materials with Schubmodule of 89.63 GPa | |
150.0 °C | 87.56 GPa Show Material materials with Schubmodule of 87.56 GPa | |
205.0 °C | 84.81 GPa Show Material materials with Schubmodule of 84.81 GPa | |
260.0 °C | 82.74 GPa Show Material materials with Schubmodule of 82.74 GPa | |
315.0 °C | 81.36 GPa Show Material materials with Schubmodule of 81.36 GPa | |
370.0 °C | 79.29 GPa Show Material materials with Schubmodule of 79.29 GPa | |
425.0 °C | 77.22 GPa Show Material materials with Schubmodule of 77.22 GPa | |
485.0 °C | 74.46 GPa Show Material materials with Schubmodule of 74.46 GPa | |
540.0 °C | 71.71 GPa Show Material materials with Schubmodule of 71.71 GPa | |
595.0 °C | 68.95 GPa Show Material materials with Schubmodule of 68.95 GPa | |
650.0 °C | 64.81 GPa Show Material materials with Schubmodule of 64.81 GPa | |
705.0 °C | 60.67 GPa Show Material materials with Schubmodule of 60.67 GPa | |
760.0 °C | 57.23 GPa Show Material materials with Schubmodule of 57.23 GPa | |
815.0 °C | 53.78 GPa Show Material materials with Schubmodule of 53.78 GPa | |
Streckgrenze | 20.0 °C | 270 MPa Show Material materials with Streckgrenze of 270 MPa |
Streckgrenze Rp 0,2 | 20.0 °C | 270 MPa Show Material materials with Streckgrenze Rp 0,2 of 270 MPa |
Streckgrenze Rp 0,2, transversal | 20.0 °C | 270 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 270 MPa |
Streckgrenze, transversal | 20.0 °C | 270 MPa Show Material materials with Streckgrenze, transversal of 270 MPa |
Zugfestigkeit | 20.0 °C | 450 - 600 MPa Show Material materials with Zugfestigkeit of 450 - 600 MPa |
Zugfestigkeit, transversal | 20.0 °C | 450 - 600 MPa Show Material materials with Zugfestigkeit, transversal of 450 - 600 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100.0 °C | 9.2E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 9.2E-6 1/K | |
20.0 °C | 9.9E-6 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 9.9E-6 1/K | ||
100.0 °C | 1E-5 - 1.03E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1E-5 - 1.03E-5 1/K | ||
200.0 °C | 1E-5 - 1.08E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1E-5 - 1.08E-5 1/K | ||
300.0 °C | 1.05E-5 - 1.12E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05E-5 - 1.12E-5 1/K | ||
400.0 °C | 1.05E-5 - 1.16E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05E-5 - 1.16E-5 1/K | ||
500.0 °C | 1.1E-5 - 1.19E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.1E-5 - 1.19E-5 1/K | ||
600.0 °C | 1.21E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21E-5 1/K | ||
700.0 °C | 1.24E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.24E-5 1/K | ||
800.0 °C | 1.29E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.29E-5 1/K | ||
900.0 °C | 1.34E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.34E-5 1/K | ||
1000.0 °C | 1.39E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.39E-5 1/K | ||
Max. Betriebstemperatur, lang | 0 - 300 °C Show Material materials with Max. Betriebstemperatur, lang of 0 - 300 °C | ||
Schmelzpunkt | 1425 - 1530 °C Show Material materials with Schmelzpunkt of 1425 - 1530 °C | Typical for Ferritic Stainless Steel | |
Spezifische Wärmekapazität | 20.0 °C | 450 - 460 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 450 - 460 J/(kg·K) | |
100.0 °C | 482 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 482 J/(kg·K) | ||
200.0 °C | 506 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 506 J/(kg·K) | ||
300.0 °C | 525 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 525 J/(kg·K) | ||
400.0 °C | 547 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 547 J/(kg·K) | ||
500.0 °C | 576 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 576 J/(kg·K) | ||
600.0 °C | 616 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 616 J/(kg·K) | ||
Temperaturleitfähigkeit | 20.0 °C | 5.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.7 mm²/s | |
Wärmeleitfähigkeit | 20.0 °C | 19.6 - 25 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 19.6 - 25 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 6E-7 - 6.17E-7 Ω·m Show Material materials with spezifischer Widerstand of 6E-7 - 6.17E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.1 - 0.3 % Show Material materials with Aluminium of 0.1 - 0.3 % |
Chrom | 15.5 - 18 % Show Material materials with Chrom of 15.5 - 18 % |
Kohlenstoff | 0.08 % Show Material materials with Kohlenstoff of 0.08 % |
Mangan | 1 % Show Material materials with Mangan of 1 % |
Phosphor | 0.04 - 0.05 % Show Material materials with Phosphor of 0.04 - 0.05 % |
Schwefel | 0.015 - 0.03 % Show Material materials with Schwefel of 0.015 - 0.03 % |
Silizium | 1 % Show Material materials with Silizium of 1 % |