Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.5 g/cm³ Show Material materials with Dichte of 8.5 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 10 % Show Material materials with Dehnung of 10 % | |
Elastizitätsmodul | 23.0 °C | 120 - 156 GPa Show Material materials with Elastizitätsmodul of 120 - 156 GPa | Typical for Nickel Copper Alloy |
Härte, Brinell | 20.0 °C | 220 [-] Show Material materials with Härte, Brinell of 220 [-] | |
Streckgrenze Rp 0,2 | 20.0 °C | 350 MPa Show Material materials with Streckgrenze Rp 0,2 of 350 MPa | |
Zugfestigkeit | 20.0 °C | 650 MPa Show Material materials with Zugfestigkeit of 650 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.1E-5 - 1.6E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.1E-5 - 1.6E-5 1/K | Typical for Nickel Copper Alloy |
Schmelzpunkt | 1170 - 1365 °C Show Material materials with Schmelzpunkt of 1170 - 1365 °C | Typical for Nickel Copper Alloy | |
Spezifische Wärmekapazität | 23.0 °C | 418 - 540 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 418 - 540 J/(kg·K) | Typical for Nickel Copper Alloy |
Wärmeleitfähigkeit | 23.0 °C | 16 - 45 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 16 - 45 W/(m·K) | Typical for Nickel Copper Alloy |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.5 - 1.5 % Show Material materials with Aluminium of 0.5 - 1.5 % |
Blei | 0.01 % Show Material materials with Blei of 0.01 % |
Eisen | 1 - 2.5 % Show Material materials with Eisen of 1 - 2.5 % |
Kohlenstoff | 0.25 % Show Material materials with Kohlenstoff of 0.25 % |
Kupfer | 27 - 33 % Show Material materials with Kupfer of 27 - 33 % |
Magnesium | 0.12 % Show Material materials with Magnesium of 0.12 % |
Nickel | 61 - 68 % Show Material materials with Nickel of 61 - 68 % |
Schwefel | 0.01 % Show Material materials with Schwefel of 0.01 % |
Silizium | 2.7 - 3.7 % Show Material materials with Silizium of 2.7 - 3.7 % |
Titan | 0.2 % Show Material materials with Titan of 0.2 % |
Technological properties
Property | ||
---|---|---|
Processing methods | sand casting, separately cast test sample |