Allgemein
Property | Value | Comment |
---|---|---|
Carbon equivalent (CET) | 0.38 [-] Show Material materials with Carbon equivalent (CET) of 0.38 [-] | max. for t ≤ 50 mm plate thickness |
0.4 [-] Show Material materials with Carbon equivalent (CET) of 0.4 [-] | max. for 50 < t ≤ 100 mm plate thickness | |
Dichte | 7.8 - 7.9 g/cm³ Show Material materials with Dichte of 7.8 - 7.9 g/cm³ | typical for low carbon steel |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Charpy impact energy, V-notch | -40 °C | 34 J Show Material materials with Charpy impact energy, V-notch of 34 J | for t ≤ 50 mm plate thickness | average |
-40 °C | 41 J Show Material materials with Charpy impact energy, V-notch of 41 J | for 50 < t ≤ 70 mm plate thickness | average | |
-40 °C | 50 J Show Material materials with Charpy impact energy, V-notch of 50 J | for 70 < t ≤ 100 mm plate thickness | average | |
Charpy impact energy, V-notch, transverse | -40 °C | 24 J Show Material materials with Charpy impact energy, V-notch, transverse of 24 J | for t ≤ 50 mm plate thickness | average |
-40 °C | 27 J Show Material materials with Charpy impact energy, V-notch, transverse of 27 J | for 50 < t ≤ 70 mm plate thickness | average | |
-40 °C | 34 J Show Material materials with Charpy impact energy, V-notch, transverse of 34 J | for 70 < t ≤ 100 mm plate thickness | average | |
Dehnung | 21 % Show Material materials with Dehnung of 21 % | min. | |
Elastizitätsmodul | 200 - 215 GPa Show Material materials with Elastizitätsmodul of 200 - 215 GPa | typical for low carbon steel | |
Poissonzahl | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | typical for low carbon steel | |
Schubmodule | 82 GPa Show Material materials with Schubmodule of 82 GPa | typical for low carbon steel | |
Zugfestigkeit | 490 - 620 MPa Show Material materials with Zugfestigkeit of 490 - 620 MPa |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 1.32e-05 - 1.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 - 1.38e-05 1/K | typical for low carbon steel |
Max. Betriebstemperatur | 500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | typical for carbon steel |
Schmelzpunkt | 1480 - 1526 °C Show Material materials with Schmelzpunkt of 1480 - 1526 °C | typical for low carbon steel |
Spezifische Wärmekapazität | 465 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 465 J/(kg·K) | typical for low carbon steel |
Wärmeleitfähigkeit | 25 - 93 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 25 - 93 W/(m·K) | typical for low carbon steel |
Elektrisch
Property | Value | Comment |
---|---|---|
spezifischer Widerstand | 1.43e-07 - 1.74e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.43e-07 - 1.74e-07 Ω·m | typical for carbon steel |
Chemical properties
Property | Value | Comment |
---|---|---|
Aluminium | 0.015 % Show Material materials with Aluminium of 0.015 % | min. |
Chrom | 0.2 % Show Material materials with Chrom of 0.2 % | max. |
Kalzium | 0.005 % Show Material materials with Kalzium of 0.005 % | max. |
Kohlenstoff | 0.18 % Show Material materials with Kohlenstoff of 0.18 % | max. |
Kupfer | 0.35 % Show Material materials with Kupfer of 0.35 % | max. |
Mangan | 0.9 - 1.6 % Show Material materials with Mangan of 0.9 - 1.6 % | |
Molybdän | 0.08 % Show Material materials with Molybdän of 0.08 % | max. |
Nickel | 0.4 % Show Material materials with Nickel of 0.4 % | max. |
Niobium | 0.02 - 0.05 % Show Material materials with Niobium of 0.02 - 0.05 % | |
Phosphor | 0.035 % Show Material materials with Phosphor of 0.035 % | max. |
Schwefel | 0.035 % Show Material materials with Schwefel of 0.035 % | max. |
Silizium | 0.1 - 0.5 % Show Material materials with Silizium of 0.1 - 0.5 % | |
Titan | 0.02 % Show Material materials with Titan of 0.02 % | max. |
Vanadium | 0.05 - 0.1 % Show Material materials with Vanadium of 0.05 - 0.1 % |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |