Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 7.84 g/cm³ Show Material materials with Dichte of 7.84 g/cm³ |
50.0 °C | 7.84 g/cm³ Show Material materials with Dichte of 7.84 g/cm³ | |
100.0 °C | 7.82 g/cm³ Show Material materials with Dichte of 7.82 g/cm³ | |
150.0 °C | 7.81 g/cm³ Show Material materials with Dichte of 7.81 g/cm³ | |
200.0 °C | 7.79 g/cm³ Show Material materials with Dichte of 7.79 g/cm³ | |
250.0 °C | 7.78 g/cm³ Show Material materials with Dichte of 7.78 g/cm³ | |
300.0 °C | 7.76 g/cm³ Show Material materials with Dichte of 7.76 g/cm³ | |
350.0 °C | 7.74 g/cm³ Show Material materials with Dichte of 7.74 g/cm³ | |
400.0 °C | 7.72 g/cm³ Show Material materials with Dichte of 7.72 g/cm³ | |
450.0 °C | 7.71 g/cm³ Show Material materials with Dichte of 7.71 g/cm³ | |
500.0 °C | 7.69 g/cm³ Show Material materials with Dichte of 7.69 g/cm³ | |
550.0 °C | 7.67 g/cm³ Show Material materials with Dichte of 7.67 g/cm³ | |
600.0 °C | 7.65 g/cm³ Show Material materials with Dichte of 7.65 g/cm³ | |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 18 - 20 % Show Material materials with Dehnung of 18 - 20 % |
Dehnung, transversal | 20.0 °C | 18 % Show Material materials with Dehnung, transversal of 18 % |
Elastizitätsmodul | -100.0 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa |
20.0 °C | 212 - 212.78 GPa Show Material materials with Elastizitätsmodul of 212 - 212.78 GPa | |
50.0 °C | 211.5 GPa Show Material materials with Elastizitätsmodul of 211.5 GPa | |
100.0 °C | 207 - 209 GPa Show Material materials with Elastizitätsmodul of 207 - 209 GPa | |
150.0 °C | 205.23 GPa Show Material materials with Elastizitätsmodul of 205.23 GPa | |
200.0 °C | 199 - 202 GPa Show Material materials with Elastizitätsmodul of 199 - 202 GPa | |
250.0 °C | 197.77 GPa Show Material materials with Elastizitätsmodul of 197.77 GPa | |
300.0 °C | 192 - 194 GPa Show Material materials with Elastizitätsmodul of 192 - 194 GPa | |
350.0 °C | 189.92 GPa Show Material materials with Elastizitätsmodul of 189.92 GPa | |
400.0 °C | 184 - 186.1 GPa Show Material materials with Elastizitätsmodul of 184 - 186.1 GPa | |
450.0 °C | 181.98 GPa Show Material materials with Elastizitätsmodul of 181.98 GPa | |
500.0 °C | 175 - 178 GPa Show Material materials with Elastizitätsmodul of 175 - 178 GPa | |
550.0 °C | 173.74 GPa Show Material materials with Elastizitätsmodul of 173.74 GPa | |
600.0 °C | 164 - 169.42 GPa Show Material materials with Elastizitätsmodul of 164 - 169.42 GPa | |
Härte, Brinell | 20.0 °C | 145 - 190 [-] Show Material materials with Härte, Brinell of 145 - 190 [-] |
Poissonzahl | 20.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] |
50.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
100.0 °C | 0.28 [-] Show Material materials with Poissonzahl of 0.28 [-] | |
150.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
200.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
250.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
300.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | |
350.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | |
400.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | |
450.0 °C | 0.31 [-] Show Material materials with Poissonzahl of 0.31 [-] | |
500.0 °C | 0.31 [-] Show Material materials with Poissonzahl of 0.31 [-] | |
550.0 °C | 0.32 [-] Show Material materials with Poissonzahl of 0.32 [-] | |
600.0 °C | 0.32 [-] Show Material materials with Poissonzahl of 0.32 [-] | |
Schubmodule | 20.0 °C | 82.8 GPa Show Material materials with Schubmodule of 82.8 GPa |
50.0 °C | 82.31 GPa Show Material materials with Schubmodule of 82.31 GPa | |
100.0 °C | 81.23 GPa Show Material materials with Schubmodule of 81.23 GPa | |
150.0 °C | 79.76 GPa Show Material materials with Schubmodule of 79.76 GPa | |
200.0 °C | 78.28 GPa Show Material materials with Schubmodule of 78.28 GPa | |
250.0 °C | 76.62 GPa Show Material materials with Schubmodule of 76.62 GPa | |
300.0 °C | 74.85 GPa Show Material materials with Schubmodule of 74.85 GPa | |
350.0 °C | 73.18 GPa Show Material materials with Schubmodule of 73.18 GPa | |
400.0 °C | 71.42 GPa Show Material materials with Schubmodule of 71.42 GPa | |
450.0 °C | 69.65 GPa Show Material materials with Schubmodule of 69.65 GPa | |
500.0 °C | 67.79 GPa Show Material materials with Schubmodule of 67.79 GPa | |
550.0 °C | 66.02 GPa Show Material materials with Schubmodule of 66.02 GPa | |
600.0 °C | 64.16 GPa Show Material materials with Schubmodule of 64.16 GPa | |
Streckgrenze Rp 0,2 | 20.0 °C | 300 - 320 MPa Show Material materials with Streckgrenze Rp 0,2 of 300 - 320 MPa |
100.0 °C | 280 - 300 MPa Show Material materials with Streckgrenze Rp 0,2 of 280 - 300 MPa | |
150.0 °C | 265 - 285 MPa Show Material materials with Streckgrenze Rp 0,2 of 265 - 285 MPa | |
200.0 °C | 250 - 270 MPa Show Material materials with Streckgrenze Rp 0,2 of 250 - 270 MPa | |
250.0 °C | 235 - 255 MPa Show Material materials with Streckgrenze Rp 0,2 of 235 - 255 MPa | |
300.0 °C | 210 - 230 MPa Show Material materials with Streckgrenze Rp 0,2 of 210 - 230 MPa | |
350.0 °C | 195 - 215 MPa Show Material materials with Streckgrenze Rp 0,2 of 195 - 215 MPa | |
400.0 °C | 180 - 200 MPa Show Material materials with Streckgrenze Rp 0,2 of 180 - 200 MPa | |
450.0 °C | 165 - 185 MPa Show Material materials with Streckgrenze Rp 0,2 of 165 - 185 MPa | |
500.0 °C | 150 - 170 MPa Show Material materials with Streckgrenze Rp 0,2 of 150 - 170 MPa | |
Streckgrenze Rp 0,2, transversal | 20.0 °C | 310 - 320 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 310 - 320 MPa |
Zugfestigkeit | 20.0 °C | 460 - 690 MPa Show Material materials with Zugfestigkeit of 460 - 690 MPa |
Zugfestigkeit, transversal | 20.0 °C | 460 - 610 MPa Show Material materials with Zugfestigkeit, transversal of 460 - 610 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100.0 °C | 1.05E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 - 1.22E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21E-5 - 1.22E-5 1/K | ||
200.0 °C | 1.27E-5 - 1.29E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27E-5 - 1.29E-5 1/K | ||
300.0 °C | 1.32E-5 - 1.34E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32E-5 - 1.34E-5 1/K | ||
400.0 °C | 1.36E-5 - 1.4E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36E-5 - 1.4E-5 1/K | ||
500.0 °C | 1.4E-5 - 1.43E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4E-5 - 1.43E-5 1/K | ||
600.0 °C | 1.44E-5 - 1.46E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.44E-5 - 1.46E-5 1/K | ||
Max. Betriebstemperatur, lang | 400 - 550 °C Show Material materials with Max. Betriebstemperatur, lang of 400 - 550 °C | ||
Schmelzpunkt | 1382 - 1529 °C Show Material materials with Schmelzpunkt of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Spezifische Wärmekapazität | -100.0 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | ||
100.0 °C | 479 - 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 - 500 J/(kg·K) | ||
200.0 °C | 499 - 540 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 - 540 J/(kg·K) | ||
300.0 °C | 517 - 580 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 - 580 J/(kg·K) | ||
400.0 °C | 536 - 620 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 - 620 J/(kg·K) | ||
500.0 °C | 558 - 690 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 - 690 J/(kg·K) | ||
600.0 °C | 587 - 780 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 - 780 J/(kg·K) | ||
Temperaturleitfähigkeit | 20.0 °C | 12.8 mm²/s Show Material materials with Temperaturleitfähigkeit of 12.8 mm²/s | |
100.0 °C | 12.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 12.1 mm²/s | ||
200.0 °C | 11.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 11.1 mm²/s | ||
300.0 °C | 10 mm²/s Show Material materials with Temperaturleitfähigkeit of 10 mm²/s | ||
400.0 °C | 8.8 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.8 mm²/s | ||
500.0 °C | 7.4 mm²/s Show Material materials with Temperaturleitfähigkeit of 7.4 mm²/s | ||
600.0 °C | 4.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.7 mm²/s | ||
Wärmeleitfähigkeit | 20.0 °C | 46.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 46.3 W/(m·K) | |
100.0 °C | 47 - 47.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 47 - 47.1 W/(m·K) | ||
200.0 °C | 46 - 46.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 46 - 46.2 W/(m·K) | ||
300.0 °C | 44 - 44.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 44 - 44.1 W/(m·K) | ||
400.0 °C | 41 - 41.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 41 - 41.3 W/(m·K) | ||
500.0 °C | 38.6 - 39 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38.6 - 39 W/(m·K) | ||
600.0 °C | 35.9 - 36 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 35.9 - 36 W/(m·K) | ||
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 2.25E-7 Ω·m Show Material materials with spezifischer Widerstand of 2.25E-7 Ω·m |
50.0 °C | 2.41E-7 Ω·m Show Material materials with spezifischer Widerstand of 2.41E-7 Ω·m | |
100.0 °C | 2.7E-7 - 2.72E-7 Ω·m Show Material materials with spezifischer Widerstand of 2.7E-7 - 2.72E-7 Ω·m | |
150.0 °C | 3.04E-7 Ω·m Show Material materials with spezifischer Widerstand of 3.04E-7 Ω·m | |
200.0 °C | 3.4E-7 - 3.42E-7 Ω·m Show Material materials with spezifischer Widerstand of 3.4E-7 - 3.42E-7 Ω·m | |
250.0 °C | 3.83E-7 Ω·m Show Material materials with spezifischer Widerstand of 3.83E-7 Ω·m | |
300.0 °C | 4.26E-7 - 4.3E-7 Ω·m Show Material materials with spezifischer Widerstand of 4.26E-7 - 4.3E-7 Ω·m | |
350.0 °C | 4.74E-7 Ω·m Show Material materials with spezifischer Widerstand of 4.74E-7 Ω·m | |
400.0 °C | 5.26E-7 - 5.3E-7 Ω·m Show Material materials with spezifischer Widerstand of 5.26E-7 - 5.3E-7 Ω·m | |
450.0 °C | 5.83E-7 Ω·m Show Material materials with spezifischer Widerstand of 5.83E-7 Ω·m | |
500.0 °C | 6.4E-7 Ω·m Show Material materials with spezifischer Widerstand of 6.4E-7 Ω·m | |
550.0 °C | 7.04E-7 Ω·m Show Material materials with spezifischer Widerstand of 7.04E-7 Ω·m | |
600.0 °C | 7.7E-7 - 7.73E-7 Ω·m Show Material materials with spezifischer Widerstand of 7.7E-7 - 7.73E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Chrom | 0.3 - 0.6 % Show Material materials with Chrom of 0.3 - 0.6 % |
Kohlenstoff | 0.1 - 0.18 % Show Material materials with Kohlenstoff of 0.1 - 0.18 % |
Mangan | 0.4 - 0.7 % Show Material materials with Mangan of 0.4 - 0.7 % |
Molybdän | 0.5 - 0.7 % Show Material materials with Molybdän of 0.5 - 0.7 % |
Phosphor | 0.04 % Show Material materials with Phosphor of 0.04 % |
Schwefel | 0.03 % Show Material materials with Schwefel of 0.03 % |
Silizium | 0.1 - 0.4 % Show Material materials with Silizium of 0.1 - 0.4 % |
Vanadium | 0.22 - 0.32 % Show Material materials with Vanadium of 0.22 - 0.32 % |