Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 7.75 - 7.76 g/cm³ Show Material materials with Dichte of 7.75 - 7.76 g/cm³ |
50.0 °C | 7.75 g/cm³ Show Material materials with Dichte of 7.75 g/cm³ | |
100.0 °C | 7.74 g/cm³ Show Material materials with Dichte of 7.74 g/cm³ | |
150.0 °C | 7.73 g/cm³ Show Material materials with Dichte of 7.73 g/cm³ | |
200.0 °C | 7.71 g/cm³ Show Material materials with Dichte of 7.71 g/cm³ | |
250.0 °C | 7.7 g/cm³ Show Material materials with Dichte of 7.7 g/cm³ | |
300.0 °C | 7.68 g/cm³ Show Material materials with Dichte of 7.68 g/cm³ | |
350.0 °C | 7.67 g/cm³ Show Material materials with Dichte of 7.67 g/cm³ | |
400.0 °C | 7.65 g/cm³ Show Material materials with Dichte of 7.65 g/cm³ | |
450.0 °C | 7.64 g/cm³ Show Material materials with Dichte of 7.64 g/cm³ | |
500.0 °C | 7.62 g/cm³ Show Material materials with Dichte of 7.62 g/cm³ | |
550.0 °C | 7.61 g/cm³ Show Material materials with Dichte of 7.61 g/cm³ | |
600.0 °C | 7.59 g/cm³ Show Material materials with Dichte of 7.59 g/cm³ | |
Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 14 - 17 % Show Material materials with Dehnung of 14 - 17 % |
Dehnung, transversal | 20.0 °C | 14 % Show Material materials with Dehnung, transversal of 14 % |
Elastizitätsmodul | 20.0 °C | 217.68 - 218 GPa Show Material materials with Elastizitätsmodul of 217.68 - 218 GPa |
50.0 °C | 216.02 GPa Show Material materials with Elastizitätsmodul of 216.02 GPa | |
100.0 °C | 212.98 - 213 GPa Show Material materials with Elastizitätsmodul of 212.98 - 213 GPa | |
150.0 °C | 209.64 GPa Show Material materials with Elastizitätsmodul of 209.64 GPa | |
200.0 °C | 206 - 206.21 GPa Show Material materials with Elastizitätsmodul of 206 - 206.21 GPa | |
250.0 °C | 202.38 GPa Show Material materials with Elastizitätsmodul of 202.38 GPa | |
300.0 °C | 198 - 198.26 GPa Show Material materials with Elastizitätsmodul of 198 - 198.26 GPa | |
350.0 °C | 193.94 GPa Show Material materials with Elastizitätsmodul of 193.94 GPa | |
400.0 °C | 189 - 190 GPa Show Material materials with Elastizitätsmodul of 189 - 190 GPa | |
450.0 °C | 184.33 GPa Show Material materials with Elastizitätsmodul of 184.33 GPa | |
500.0 °C | 178.93 - 180 GPa Show Material materials with Elastizitätsmodul of 178.93 - 180 GPa | |
550.0 °C | 172.85 GPa Show Material materials with Elastizitätsmodul of 172.85 GPa | |
600.0 °C | 165.79 - 167 GPa Show Material materials with Elastizitätsmodul of 165.79 - 167 GPa | |
Poissonzahl | 20.0 °C | 0.28 [-] Show Material materials with Poissonzahl of 0.28 [-] |
50.0 °C | 0.28 [-] Show Material materials with Poissonzahl of 0.28 [-] | |
100.0 °C | 0.28 [-] Show Material materials with Poissonzahl of 0.28 [-] | |
150.0 °C | 0.28 [-] Show Material materials with Poissonzahl of 0.28 [-] | |
200.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
250.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
300.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
350.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | |
400.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | |
450.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | |
500.0 °C | 0.31 [-] Show Material materials with Poissonzahl of 0.31 [-] | |
550.0 °C | 0.31 [-] Show Material materials with Poissonzahl of 0.31 [-] | |
600.0 °C | 0.31 [-] Show Material materials with Poissonzahl of 0.31 [-] | |
Schubmodule | 20.0 °C | 84.95 GPa Show Material materials with Schubmodule of 84.95 GPa |
50.0 °C | 84.27 GPa Show Material materials with Schubmodule of 84.27 GPa | |
100.0 °C | 82.99 GPa Show Material materials with Schubmodule of 82.99 GPa | |
150.0 °C | 81.62 GPa Show Material materials with Schubmodule of 81.62 GPa | |
200.0 °C | 80.05 GPa Show Material materials with Schubmodule of 80.05 GPa | |
250.0 °C | 78.48 GPa Show Material materials with Schubmodule of 78.48 GPa | |
300.0 °C | 76.71 GPa Show Material materials with Schubmodule of 76.71 GPa | |
350.0 °C | 74.95 GPa Show Material materials with Schubmodule of 74.95 GPa | |
400.0 °C | 73.08 GPa Show Material materials with Schubmodule of 73.08 GPa | |
450.0 °C | 70.93 GPa Show Material materials with Schubmodule of 70.93 GPa | |
500.0 °C | 68.57 GPa Show Material materials with Schubmodule of 68.57 GPa | |
550.0 °C | 66.02 GPa Show Material materials with Schubmodule of 66.02 GPa | |
600.0 °C | 63.27 GPa Show Material materials with Schubmodule of 63.27 GPa | |
Streckgrenze Rp 0,2 | 20.0 °C | 490 - 500 MPa Show Material materials with Streckgrenze Rp 0,2 of 490 - 500 MPa |
100.0 °C | 460 MPa Show Material materials with Streckgrenze Rp 0,2 of 460 MPa | |
150.0 °C | 445 MPa Show Material materials with Streckgrenze Rp 0,2 of 445 MPa | |
200.0 °C | 430 MPa Show Material materials with Streckgrenze Rp 0,2 of 430 MPa | |
250.0 °C | 415 MPa Show Material materials with Streckgrenze Rp 0,2 of 415 MPa | |
300.0 °C | 390 MPa Show Material materials with Streckgrenze Rp 0,2 of 390 MPa | |
350.0 °C | 380 MPa Show Material materials with Streckgrenze Rp 0,2 of 380 MPa | |
400.0 °C | 360 MPa Show Material materials with Streckgrenze Rp 0,2 of 360 MPa | |
450.0 °C | 330 MPa Show Material materials with Streckgrenze Rp 0,2 of 330 MPa | |
500.0 °C | 290 MPa Show Material materials with Streckgrenze Rp 0,2 of 290 MPa | |
550.0 °C | 250 MPa Show Material materials with Streckgrenze Rp 0,2 of 250 MPa | |
600.0 °C | 160 MPa Show Material materials with Streckgrenze Rp 0,2 of 160 MPa | |
Streckgrenze Rp 0,2, transversal | 20.0 °C | 490 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 490 MPa |
Zugfestigkeit | 20.0 °C | 690 - 850 MPa Show Material materials with Zugfestigkeit of 690 - 850 MPa |
Zugfestigkeit, transversal | 20.0 °C | 690 - 840 MPa Show Material materials with Zugfestigkeit, transversal of 690 - 840 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20.0 °C | 1.02E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.02E-5 1/K | |
100.0 °C | 1.05E-5 - 1.08E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05E-5 - 1.08E-5 1/K | ||
200.0 °C | 1.09E-5 - 1.12E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.09E-5 - 1.12E-5 1/K | ||
300.0 °C | 1.13E-5 - 1.16E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.13E-5 - 1.16E-5 1/K | ||
400.0 °C | 1.16E-5 - 1.19E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.16E-5 - 1.19E-5 1/K | ||
500.0 °C | 1.2E-5 - 1.21E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.2E-5 - 1.21E-5 1/K | ||
600.0 °C | 1.22E-5 - 1.23E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.22E-5 - 1.23E-5 1/K | ||
Max. Betriebstemperatur, lang | 0 - 580 °C Show Material materials with Max. Betriebstemperatur, lang of 0 - 580 °C | ||
Schmelzpunkt | 1370 - 1530 °C Show Material materials with Schmelzpunkt of 1370 - 1530 °C | Typical for Martensitic Stainless Steel | |
Spezifische Wärmekapazität | 20.0 °C | 439 - 460 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 439 - 460 J/(kg·K) | |
100.0 °C | 474 - 490 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 474 - 490 J/(kg·K) | ||
200.0 °C | 498 - 540 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 498 - 540 J/(kg·K) | ||
300.0 °C | 517 - 580 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 - 580 J/(kg·K) | ||
400.0 °C | 538 - 630 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 538 - 630 J/(kg·K) | ||
500.0 °C | 564 - 710 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 564 - 710 J/(kg·K) | ||
600.0 °C | 598 - 830 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 598 - 830 J/(kg·K) | ||
Temperaturleitfähigkeit | 20.0 °C | 7.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 7.1 mm²/s | |
100.0 °C | 6.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 6.3 mm²/s | ||
200.0 °C | 6 mm²/s Show Material materials with Temperaturleitfähigkeit of 6 mm²/s | ||
300.0 °C | 5.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.7 mm²/s | ||
400.0 °C | 5.4 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.4 mm²/s | ||
500.0 °C | 4.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.9 mm²/s | ||
600.0 °C | 4.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 4.1 mm²/s | ||
Wärmeleitfähigkeit | 20.0 °C | 24 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 24 W/(m·K) | |
100.0 °C | 24 - 24.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 24 - 24.4 W/(m·K) | ||
200.0 °C | 24.8 - 25 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 24.8 - 25 W/(m·K) | ||
300.0 °C | 25 - 25.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 25 - 25.1 W/(m·K) | ||
400.0 °C | 25.6 - 26 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 25.6 - 26 W/(m·K) | ||
500.0 °C | 26 - 26.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 26 - 26.1 W/(m·K) | ||
600.0 °C | 26 - 26.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 26 - 26.4 W/(m·K) | ||
650.0 °C | 30 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 30 W/(m·K) | ||
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 6E-7 - 6.03E-7 Ω·m Show Material materials with spezifischer Widerstand of 6E-7 - 6.03E-7 Ω·m |
50.0 °C | 6.26E-7 Ω·m Show Material materials with spezifischer Widerstand of 6.26E-7 Ω·m | |
100.0 °C | 6.68E-7 - 6.7E-7 Ω·m Show Material materials with spezifischer Widerstand of 6.68E-7 - 6.7E-7 Ω·m | |
150.0 °C | 7.06E-7 Ω·m Show Material materials with spezifischer Widerstand of 7.06E-7 Ω·m | |
200.0 °C | 7.4E-7 - 7.43E-7 Ω·m Show Material materials with spezifischer Widerstand of 7.4E-7 - 7.43E-7 Ω·m | |
250.0 °C | 7.83E-7 Ω·m Show Material materials with spezifischer Widerstand of 7.83E-7 Ω·m | |
300.0 °C | 8.17E-7 - 8.2E-7 Ω·m Show Material materials with spezifischer Widerstand of 8.17E-7 - 8.2E-7 Ω·m | |
350.0 °C | 8.54E-7 Ω·m Show Material materials with spezifischer Widerstand of 8.54E-7 Ω·m | |
400.0 °C | 8.9E-7 Ω·m Show Material materials with spezifischer Widerstand of 8.9E-7 Ω·m | |
450.0 °C | 9.25E-7 Ω·m Show Material materials with spezifischer Widerstand of 9.25E-7 Ω·m | |
500.0 °C | 9.6E-7 - 9.62E-7 Ω·m Show Material materials with spezifischer Widerstand of 9.6E-7 - 9.62E-7 Ω·m | |
550.0 °C | 9.99E-7 Ω·m Show Material materials with spezifischer Widerstand of 9.99E-7 Ω·m | |
600.0 °C | 1.03E-6 - 1.04E-6 Ω·m Show Material materials with spezifischer Widerstand of 1.03E-6 - 1.04E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Chrom | 10 - 12.5 % Show Material materials with Chrom of 10 - 12.5 % |
Kohlenstoff | 0.17 - 0.23 % Show Material materials with Kohlenstoff of 0.17 - 0.23 % |
Mangan | 1 % Show Material materials with Mangan of 1 % |
Molybdän | 0.8 - 1.2 % Show Material materials with Molybdän of 0.8 - 1.2 % |
Nickel | 0.3 - 0.8 % Show Material materials with Nickel of 0.3 - 0.8 % |
Phosphor | 0.03 % Show Material materials with Phosphor of 0.03 % |
Schwefel | 0.03 % Show Material materials with Schwefel of 0.03 % |
Silizium | 0.5 % Show Material materials with Silizium of 0.5 % |
Vanadium | 0.25 - 0.35 % Show Material materials with Vanadium of 0.25 - 0.35 % |