Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.84 g/cm³ Show Material materials with Dichte of 7.84 g/cm³ | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 14.9 % Show Material materials with Dehnung of 14.9 % | Predicted Value, A200 | ||||
17.0 % Show Material materials with Dehnung of 17.0 % | Predicted Value, A80 Transverse | |||||
18.0 % Show Material materials with Dehnung of 18.0 % | Predicted Value, A80 | |||||
20.4 % Show Material materials with Dehnung of 20.4 % | Predicted Value, A5 | |||||
21.0 % Show Material materials with Dehnung of 21.0 % | Predicted Value, A50 | |||||
20 °C | 18 % Show Material materials with Dehnung of 18 % | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | Transverse | |
20 °C | 20 % Show Material materials with Dehnung of 20 % | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
Elastizitätsmodul | -100 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | |
20 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
100 °C | 207 - 208 GPa Show Material materials with Elastizitätsmodul of 207 - 208 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
100 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
100 °C | 208 GPa Show Material materials with Elastizitätsmodul of 208 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
200 °C | 199 - 202 GPa Show Material materials with Elastizitätsmodul of 199 - 202 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
200 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
200 °C | 202 GPa Show Material materials with Elastizitätsmodul of 202 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
300 °C | 192 - 194 GPa Show Material materials with Elastizitätsmodul of 192 - 194 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
300 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
300 °C | 194 GPa Show Material materials with Elastizitätsmodul of 194 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
400 °C | 184 - 186 GPa Show Material materials with Elastizitätsmodul of 184 - 186 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
400 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
400 °C | 186 GPa Show Material materials with Elastizitätsmodul of 186 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
500 °C | 175 - 176 GPa Show Material materials with Elastizitätsmodul of 175 - 176 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
500 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
500 °C | 176 GPa Show Material materials with Elastizitätsmodul of 176 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
600 °C | 164 - 166 GPa Show Material materials with Elastizitätsmodul of 164 - 166 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
600 °C | 164 GPa Show Material materials with Elastizitätsmodul of 164 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
600 °C | 166 GPa Show Material materials with Elastizitätsmodul of 166 GPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
Flächenreduzierung | 46.2 % Show Material materials with Flächenreduzierung of 46.2 % | Predicted Value, Transverse | ||||
20 °C | 50 % Show Material materials with Flächenreduzierung of 50 % | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
Poissonzahl | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Chromium Molybdenum Steel | ||||
Scherfestigkeit | 631.8 MPa Show Material materials with Scherfestigkeit of 631.8 MPa | Predicted Value | ||||
Schubmodule | 81.2 GPa Show Material materials with Schubmodule of 81.2 GPa | Predicted Value | ||||
Zugfestigkeit | 20 °C | 540 - 690 MPa Show Material materials with Zugfestigkeit of 540 - 690 MPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | Transverse |
20 °C | 540 - 690 MPa Show Material materials with Zugfestigkeit of 540 - 690 MPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
100 °C | 500 MPa Show Material materials with Zugfestigkeit of 500 MPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | |||
150 °C | 480 MPa Show Material materials with Zugfestigkeit of 480 MPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | |||
200 °C | 460 MPa Show Material materials with Zugfestigkeit of 460 MPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | |||
250 °C | 450 MPa Show Material materials with Zugfestigkeit of 450 MPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | |||
300 °C | 440 MPa Show Material materials with Zugfestigkeit of 440 MPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | |||
350 °C | 430 MPa Show Material materials with Zugfestigkeit of 430 MPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | |||
400 °C | 410 MPa Show Material materials with Zugfestigkeit of 410 MPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | |||
450 °C | 380 MPa Show Material materials with Zugfestigkeit of 380 MPa | quenched and tempered (+QT) | DIN 17176, EN 10216-2 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.05e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | |
20 °C | 1.15e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.15e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
100 °C | 1.21e-05 - 1.22e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 - 1.22e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
100 °C | 1.21e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
100 °C | 1.22e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.22e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
200 °C | 1.27e-05 - 1.29e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27e-05 - 1.29e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
200 °C | 1.27e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
200 °C | 1.29e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.29e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
300 °C | 1.32e-05 - 1.34e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 - 1.34e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
300 °C | 1.32e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
300 °C | 1.34e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.34e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
400 °C | 1.36e-05 - 1.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 - 1.4e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
400 °C | 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
400 °C | 1.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
500 °C | 1.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
500 °C | 1.4e-05 - 1.43e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-05 - 1.43e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
500 °C | 1.43e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.43e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
600 °C | 1.44e-05 - 1.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.44e-05 - 1.46e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
600 °C | 1.44e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.44e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
600 °C | 1.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.46e-05 1/K | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
Schmelzpunkt | 1382 - 1529 °C Show Material materials with Schmelzpunkt of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | ||||
Spezifische Wärmekapazität | -100 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | |
20 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
100 °C | 479 - 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 - 500 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
100 °C | 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 500 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
200 °C | 499 - 540 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 - 540 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
200 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
200 °C | 540 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 540 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
300 °C | 517 - 580 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 - 580 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
300 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
300 °C | 580 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 580 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
400 °C | 536 - 620 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 - 620 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
400 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
400 °C | 620 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 620 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
500 °C | 558 - 690 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 - 690 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
500 °C | 558 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
500 °C | 690 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 690 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
600 °C | 587 - 780 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 - 780 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
600 °C | 587 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
600 °C | 780 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 780 J/(kg·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
Temperaturleitfähigkeit | 20 °C | 9.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.7 mm²/s | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | |
100 °C | 9.6 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.6 mm²/s | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
200 °C | 9.2 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.2 mm²/s | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
300 °C | 8.5 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.5 mm²/s | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
400 °C | 7.8 mm²/s Show Material materials with Temperaturleitfähigkeit of 7.8 mm²/s | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
500 °C | 6.8 mm²/s Show Material materials with Temperaturleitfähigkeit of 6.8 mm²/s | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
600 °C | 5.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.7 mm²/s | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
Wärmeleitfähigkeit | 20 °C | 34.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 34.9 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | |
100 °C | 37 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 37 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
100 °C | 37 - 37.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 37 - 37.3 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
100 °C | 37.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 37.3 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
200 °C | 38 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
200 °C | 38 - 38.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38 - 38.2 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
200 °C | 38.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38.2 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
300 °C | 37.8 - 38 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 37.8 - 38 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
300 °C | 37.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 37.8 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
300 °C | 38 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
400 °C | 36.6 - 37 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36.6 - 37 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
400 °C | 36.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36.6 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
400 °C | 37 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 37 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
500 °C | 35 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 35 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
500 °C | 35 - 35.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 35 - 35.2 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
500 °C | 35.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 35.2 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
600 °C | 33 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 33 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
600 °C | 33 - 33.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 33 - 33.6 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
600 °C | 33.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 33.6 W/(m·K) | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 3 S/m Show Material materials with Elektrische Leitfähigkeit of 3 S/m | Predicted Value | ||||
spezifischer Widerstand | 20 °C | 2.98e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.98e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | |
100 °C | 3.4e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
100 °C | 3.4e-07 - 3.43e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-07 - 3.43e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
100 °C | 3.43e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.43e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
200 °C | 4.1e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.1e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
200 °C | 4.1e-07 - 4.13e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.1e-07 - 4.13e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
200 °C | 4.13e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.13e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
300 °C | 4.97e-07 - 5e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.97e-07 - 5e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
300 °C | 4.97e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.97e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
300 °C | 5e-07 Ω·m Show Material materials with spezifischer Widerstand of 5e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
400 °C | 5.9e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.9e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
400 °C | 5.9e-07 - 5.95e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.9e-07 - 5.95e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
400 °C | 5.95e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.95e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
500 °C | 7e-07 Ω·m Show Material materials with spezifischer Widerstand of 7e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
500 °C | 7e-07 - 7.03e-07 Ω·m Show Material materials with spezifischer Widerstand of 7e-07 - 7.03e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
500 °C | 7.03e-07 Ω·m Show Material materials with spezifischer Widerstand of 7.03e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
600 °C | 8.2e-07 Ω·m Show Material materials with spezifischer Widerstand of 8.2e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
600 °C | 8.2e-07 - 8.25e-07 Ω·m Show Material materials with spezifischer Widerstand of 8.2e-07 - 8.25e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube | ||
600 °C | 8.25e-07 Ω·m Show Material materials with spezifischer Widerstand of 8.25e-07 Ω·m | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.01 % Show Material materials with Aluminium of 0.01 % | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube |
Chrom | 2 - 2.5 % Show Material materials with Chrom of 2 - 2.5 % | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube |
Kohlenstoff | 0.1 - 0.15 % Show Material materials with Kohlenstoff of 0.1 - 0.15 % | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube |
Kupfer | 0.2 % Show Material materials with Kupfer of 0.2 % | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube |
Mangan | 0.3 - 0.8 % Show Material materials with Mangan of 0.3 - 0.8 % | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube |
Molybdän | 0.9 - 1.1 % Show Material materials with Molybdän of 0.9 - 1.1 % | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube |
Nickel | 0.3 % Show Material materials with Nickel of 0.3 % | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube |
Phosphor | 0.015 % Show Material materials with Phosphor of 0.015 % | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube |
Schwefel | 0.015 % Show Material materials with Schwefel of 0.015 % | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube |
Silizium | 0.3 % Show Material materials with Silizium of 0.3 % | quenched and tempered (+QT) | DIN 17176, EN 10216-2 | Seamless Tube |