Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 7.85 g/cm³ Show Material materials with Dichte of 7.85 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 10 - 16 % Show Material materials with Dehnung of 10 - 16 % | |
Elastizitätsmodul | 20.0 °C | 211 GPa Show Material materials with Elastizitätsmodul of 211 GPa | |
100.0 °C | 204 GPa Show Material materials with Elastizitätsmodul of 204 GPa | ||
200.0 °C | 196 GPa Show Material materials with Elastizitätsmodul of 196 GPa | ||
300.0 °C | 186 GPa Show Material materials with Elastizitätsmodul of 186 GPa | ||
Poissonzahl | 20.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Nickel Chromium Molybdenum Steel |
Streckgrenze Rp 0,2 | 20.0 °C | 650 - 700 MPa Show Material materials with Streckgrenze Rp 0,2 of 650 - 700 MPa | |
Zugfestigkeit | 20.0 °C | 800 - 1000 MPa Show Material materials with Zugfestigkeit of 800 - 1000 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.1E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.1E-5 1/K | |
200.0 °C | 1.2E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.2E-5 1/K | ||
300.0 °C | 1.3E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.3E-5 1/K | ||
Max. Betriebstemperatur, lang | 0 - 300 °C Show Material materials with Max. Betriebstemperatur, lang of 0 - 300 °C | ||
Schmelzpunkt | 1382 - 1529 °C Show Material materials with Schmelzpunkt of 1382 - 1529 °C | Typical for Nickel Chromium Molybdenum Steel | |
Wärmeleitfähigkeit | 20.0 °C | 34 - 54 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 34 - 54 W/(m·K) | Typical for Nickel Chromium Molybdenum Steel |
Chemical properties
Property | Value |
---|---|
Chrom | 0.9 - 1.2 % Show Material materials with Chrom of 0.9 - 1.2 % |
Kohlenstoff | 0.3 - 0.36 % Show Material materials with Kohlenstoff of 0.3 - 0.36 % |
Mangan | 0.5 - 0.8 % Show Material materials with Mangan of 0.5 - 0.8 % |
Molybdän | 0.35 - 0.5 % Show Material materials with Molybdän of 0.35 - 0.5 % |
Nickel | 1.5 - 1.8 % Show Material materials with Nickel of 1.5 - 1.8 % |
Phosphor | 0.02 % Show Material materials with Phosphor of 0.02 % |
Schwefel | 7E-3 % Show Material materials with Schwefel of 7E-3 % |
Silizium | 0.6 % Show Material materials with Silizium of 0.6 % |