Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 7.7 g/cm³ Show Material materials with Dichte of 7.7 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 5 % Show Material materials with Dehnung of 5 % | |
Elastizitätsmodul | 23.0 °C | 220 GPa Show Material materials with Elastizitätsmodul of 220 GPa | Typical for Martensitic Stainless Steel |
Härte, Brinell | 20.0 °C | 220 - 300 [-] Show Material materials with Härte, Brinell of 220 - 300 [-] | |
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Martensitic Stainless Steel |
Schubmodule | 23.0 °C | 77 GPa Show Material materials with Schubmodule of 77 GPa | Typical for Martensitic Stainless Steel |
Streckgrenze Rp 0,2 | 20.0 °C | 600 MPa Show Material materials with Streckgrenze Rp 0,2 of 600 MPa | |
100.0 °C | 560 MPa Show Material materials with Streckgrenze Rp 0,2 of 560 MPa | ||
200.0 °C | 540 MPa Show Material materials with Streckgrenze Rp 0,2 of 540 MPa | ||
300.0 °C | 540 MPa Show Material materials with Streckgrenze Rp 0,2 of 540 MPa | ||
350.0 °C | 520 MPa Show Material materials with Streckgrenze Rp 0,2 of 520 MPa | ||
400.0 °C | 500 MPa Show Material materials with Streckgrenze Rp 0,2 of 500 MPa | ||
Zugfestigkeit | 20.0 °C | 780 - 980 MPa Show Material materials with Zugfestigkeit of 780 - 980 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.05E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05E-5 1/K | |
200.0 °C | 1.1E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.1E-5 1/K | ||
300.0 °C | 1.1E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.1E-5 1/K | ||
400.0 °C | 1.15E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.15E-5 1/K | ||
500.0 °C | 1.2E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.2E-5 1/K | ||
Schmelzpunkt | 1370 - 1530 °C Show Material materials with Schmelzpunkt of 1370 - 1530 °C | Typical for Martensitic Stainless Steel | |
Spezifische Wärmekapazität | 20.0 °C | 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 500 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 19 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 19 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 6.5E-7 Ω·m Show Material materials with spezifischer Widerstand of 6.5E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Chrom | 15.5 - 17.5 % Show Material materials with Chrom of 15.5 - 17.5 % |
Kohlenstoff | 0.33 - 0.43 % Show Material materials with Kohlenstoff of 0.33 - 0.43 % |
Mangan | 1 % Show Material materials with Mangan of 1 % |
Molybdän | 0.9 - 1.3 % Show Material materials with Molybdän of 0.9 - 1.3 % |
Nickel | 1 % Show Material materials with Nickel of 1 % |
Phosphor | 0.05 % Show Material materials with Phosphor of 0.05 % |
Schwefel | 0.03 % Show Material materials with Schwefel of 0.03 % |
Silizium | 1 % Show Material materials with Silizium of 1 % |