Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 7.9 g/cm³ Show Material materials with Dichte of 7.9 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 20 % Show Material materials with Dehnung of 20 % | |
Elastizitätsmodul | 23.0 °C | 195 GPa Show Material materials with Elastizitätsmodul of 195 GPa | Typical for Austenitic Stainless Steel |
Härte, Brinell | 20.0 °C | 130 - 200 [-] Show Material materials with Härte, Brinell of 130 - 200 [-] | |
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Austenitic Stainless Steel |
Schubmodule | 23.0 °C | 77 GPa Show Material materials with Schubmodule of 77 GPa | Typical for Austenitic Stainless Steel |
Streckgrenze Rp 0,2 | 20.0 °C | 175 MPa Show Material materials with Streckgrenze Rp 0,2 of 175 MPa | |
100.0 °C | 150 MPa Show Material materials with Streckgrenze Rp 0,2 of 150 MPa | ||
150.0 °C | 135 MPa Show Material materials with Streckgrenze Rp 0,2 of 135 MPa | ||
200.0 °C | 130 MPa Show Material materials with Streckgrenze Rp 0,2 of 130 MPa | ||
250.0 °C | 125 MPa Show Material materials with Streckgrenze Rp 0,2 of 125 MPa | ||
300.0 °C | 120 MPa Show Material materials with Streckgrenze Rp 0,2 of 120 MPa | ||
350.0 °C | 115 MPa Show Material materials with Streckgrenze Rp 0,2 of 115 MPa | ||
400.0 °C | 110 MPa Show Material materials with Streckgrenze Rp 0,2 of 110 MPa | ||
450.0 °C | 105 MPa Show Material materials with Streckgrenze Rp 0,2 of 105 MPa | ||
500.0 °C | 100 MPa Show Material materials with Streckgrenze Rp 0,2 of 100 MPa | ||
550.0 °C | 90 MPa Show Material materials with Streckgrenze Rp 0,2 of 90 MPa | ||
Streckgrenze Rp 1,0 | 20.0 °C | 200 MPa Show Material materials with Streckgrenze Rp 1,0 of 200 MPa | |
100.0 °C | 175 MPa Show Material materials with Streckgrenze Rp 1,0 of 175 MPa | ||
150.0 °C | 160 MPa Show Material materials with Streckgrenze Rp 1,0 of 160 MPa | ||
200.0 °C | 155 MPa Show Material materials with Streckgrenze Rp 1,0 of 155 MPa | ||
250.0 °C | 150 MPa Show Material materials with Streckgrenze Rp 1,0 of 150 MPa | ||
300.0 °C | 145 MPa Show Material materials with Streckgrenze Rp 1,0 of 145 MPa | ||
350.0 °C | 140 MPa Show Material materials with Streckgrenze Rp 1,0 of 140 MPa | ||
400.0 °C | 130 MPa Show Material materials with Streckgrenze Rp 1,0 of 130 MPa | ||
450.0 °C | 120 MPa Show Material materials with Streckgrenze Rp 1,0 of 120 MPa | ||
500.0 °C | 110 MPa Show Material materials with Streckgrenze Rp 1,0 of 110 MPa | ||
550.0 °C | 100 MPa Show Material materials with Streckgrenze Rp 1,0 of 100 MPa | ||
Zugfestigkeit | 20.0 °C | 440 - 640 MPa Show Material materials with Zugfestigkeit of 440 - 640 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.6E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6E-5 1/K | |
200.0 °C | 1.7E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 1/K | ||
300.0 °C | 1.7E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 1/K | ||
400.0 °C | 1.8E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.8E-5 1/K | ||
500.0 °C | 1.8E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.8E-5 1/K | ||
Max. Betriebstemperatur, lang | 0 - 550 °C Show Material materials with Max. Betriebstemperatur, lang of 0 - 550 °C | ||
Schmelzpunkt | 1230 - 1480 °C Show Material materials with Schmelzpunkt of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Spezifische Wärmekapazität | 20.0 °C | 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 500 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 15 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 15 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 5.5E-7 - 7.5E-7 Ω·m Show Material materials with spezifischer Widerstand of 5.5E-7 - 7.5E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Chrom | 18 - 20 % Show Material materials with Chrom of 18 - 20 % |
Kohlenstoff | 0.06 % Show Material materials with Kohlenstoff of 0.06 % |
Mangan | 1.5 % Show Material materials with Mangan of 1.5 % |
Nickel | 9 - 11 % Show Material materials with Nickel of 9 - 11 % |
Phosphor | 0.05 % Show Material materials with Phosphor of 0.05 % |
Schwefel | 0.03 % Show Material materials with Schwefel of 0.03 % |
Silizium | 1.5 % Show Material materials with Silizium of 1.5 % |