Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 7.7 g/cm³ Show Material materials with Dichte of 7.7 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Elastizitätsmodul | 20.0 °C | 223 GPa Show Material materials with Elastizitätsmodul of 223 GPa | |
100.0 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | ||
200.0 °C | 209 GPa Show Material materials with Elastizitätsmodul of 209 GPa | ||
300.0 °C | 201 GPa Show Material materials with Elastizitätsmodul of 201 GPa | ||
400.0 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | ||
500.0 °C | 183 GPa Show Material materials with Elastizitätsmodul of 183 GPa | ||
Härte, Brinell | 20.0 °C | 230 [-] Show Material materials with Härte, Brinell of 230 [-] | |
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Martensitic Stainless Steel |
Schubmodule | 23.0 °C | 77 GPa Show Material materials with Schubmodule of 77 GPa | Typical for Martensitic Stainless Steel |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.04E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.04E-5 1/K | |
200.0 °C | 1.08E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.08E-5 1/K | ||
300.0 °C | 1.12E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.12E-5 1/K | ||
400.0 °C | 1.16E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.16E-5 1/K | ||
500.0 °C | 1.19E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.19E-5 1/K | ||
Schmelzpunkt | 1370 - 1530 °C Show Material materials with Schmelzpunkt of 1370 - 1530 °C | Typical for Martensitic Stainless Steel | |
Spezifische Wärmekapazität | 20.0 °C | 430 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 430 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 15 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 15 W/(m·K) |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
spezifischer Widerstand | 23.0 °C | 6E-7 Ω·m Show Material materials with spezifischer Widerstand of 6E-7 Ω·m | Typical for Martensitic Stainless Steel |
Chemical properties
Property | Value |
---|---|
Chrom | 14 - 16 % Show Material materials with Chrom of 14 - 16 % |
Kohlenstoff | 0.25 - 0.35 % Show Material materials with Kohlenstoff of 0.25 - 0.35 % |
Mangan | 1 % Show Material materials with Mangan of 1 % |
Molybdän | 0.85 - 1.1 % Show Material materials with Molybdän of 0.85 - 1.1 % |
Nickel | 0.5 % Show Material materials with Nickel of 0.5 % |
Phosphor | 0.03 % Show Material materials with Phosphor of 0.03 % |
Schwefel | 0.025 % Show Material materials with Schwefel of 0.025 % |
Silizium | 1 % Show Material materials with Silizium of 1 % |
Stickstoff | 0.3 - 0.5 % Show Material materials with Stickstoff of 0.3 - 0.5 % |