Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.84 g/cm³ Show Material materials with Dichte of 7.84 g/cm³ | thermomechanically rolled | EN 10149-2 | Flat |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 14.5 % Show Material materials with Dehnung of 14.5 % | Predicted Value, A200 | ||||
16.5 % Show Material materials with Dehnung of 16.5 % | Predicted Value, Transverse | |||||
17.1 % Show Material materials with Dehnung of 17.1 % | Predicted Value, A80 Transverse | |||||
18.7 % Show Material materials with Dehnung of 18.7 % | Predicted Value, A50 | |||||
21.2 % Show Material materials with Dehnung of 21.2 % | Predicted Value, A5 | |||||
20 °C | 14 % Show Material materials with Dehnung of 14 % | thermomechanically rolled | EN 10149-2 | Flat | A80 | |
20 °C | 17 % Show Material materials with Dehnung of 17 % | thermomechanically rolled | EN 10149-2 | Flat | ||
Elastizitätsmodul | -100 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | thermomechanically rolled | EN 10149-2 | Flat | |
20 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | thermomechanically rolled | EN 10149-2 | Flat | ||
100 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | thermomechanically rolled | EN 10149-2 | Flat | ||
200 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | thermomechanically rolled | EN 10149-2 | Flat | ||
300 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | thermomechanically rolled | EN 10149-2 | Flat | ||
400 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | thermomechanically rolled | EN 10149-2 | Flat | ||
500 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | thermomechanically rolled | EN 10149-2 | Flat | ||
600 °C | 164 GPa Show Material materials with Elastizitätsmodul of 164 GPa | thermomechanically rolled | EN 10149-2 | Flat | ||
Flächenreduzierung | 39.3 % Show Material materials with Flächenreduzierung of 39.3 % | Predicted Value | ||||
44.1 % Show Material materials with Flächenreduzierung of 44.1 % | Predicted Value, Transverse | |||||
Härte, Brinell | 243 [-] Show Material materials with Härte, Brinell of 243 [-] | Predicted Value, Transverse | ||||
Poissonzahl | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Low Carbon Steel | ||||
Scherfestigkeit | 500.8 MPa Show Material materials with Scherfestigkeit of 500.8 MPa | Predicted Value | ||||
Schubmodule | 82 GPa Show Material materials with Schubmodule of 82 GPa | Typical for Low Carbon Steel | ||||
Streckgrenze | 252.3 MPa Show Material materials with Streckgrenze of 252.3 MPa | Predicted Value, RP1 | ||||
298.7 MPa Show Material materials with Streckgrenze of 298.7 MPa | Predicted Value, RP1 Transverse | |||||
399.3 MPa Show Material materials with Streckgrenze of 399.3 MPa | Predicted Value, Transverse | |||||
451.1 MPa Show Material materials with Streckgrenze of 451.1 MPa | Predicted Value, RP02 | |||||
466 MPa Show Material materials with Streckgrenze of 466 MPa | Predicted Value, RP05 | |||||
481.6 MPa Show Material materials with Streckgrenze of 481.6 MPa | Predicted Value, RP02 Transverse | |||||
516.2 MPa Show Material materials with Streckgrenze of 516.2 MPa | Predicted Value, RP002 | |||||
20 °C | 460 MPa Show Material materials with Streckgrenze of 460 MPa | thermomechanically rolled | EN 10149-2 | Flat | ||
Zugfestigkeit | 20 °C | 520 - 670 MPa Show Material materials with Zugfestigkeit of 520 - 670 MPa | thermomechanically rolled | EN 10149-2 | Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.08e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.08e-05 1/K | thermomechanically rolled | EN 10149-2 | Flat | |
20 °C | 1.19e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.19e-05 1/K | thermomechanically rolled | EN 10149-2 | Flat | ||
100 °C | 1.25e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.25e-05 1/K | thermomechanically rolled | EN 10149-2 | Flat | ||
200 °C | 1.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.3e-05 1/K | thermomechanically rolled | EN 10149-2 | Flat | ||
300 °C | 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | thermomechanically rolled | EN 10149-2 | Flat | ||
400 °C | 1.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.41e-05 1/K | thermomechanically rolled | EN 10149-2 | Flat | ||
500 °C | 1.45e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.45e-05 1/K | thermomechanically rolled | EN 10149-2 | Flat | ||
600 °C | 1.49e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.49e-05 1/K | thermomechanically rolled | EN 10149-2 | Flat | ||
Max. Betriebstemperatur | -20 °C Show Material materials with Max. Betriebstemperatur of -20 °C | thermomechanically rolled | EN 10149-2 | Flat | Long | |
500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | Typical for Carbon Steel | |||||
Schmelzpunkt | 1480 - 1526 °C Show Material materials with Schmelzpunkt of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Spezifische Wärmekapazität | -100 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | thermomechanically rolled | EN 10149-2 | Flat | |
20 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 J/(kg·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 J/(kg·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
Temperaturleitfähigkeit | -100 °C | 15.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 15.9 mm²/s | thermomechanically rolled | EN 10149-2 | Flat | |
20 °C | 13.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 13.7 mm²/s | thermomechanically rolled | EN 10149-2 | Flat | ||
100 °C | 12.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 12.7 mm²/s | thermomechanically rolled | EN 10149-2 | Flat | ||
200 °C | 11.5 mm²/s Show Material materials with Temperaturleitfähigkeit of 11.5 mm²/s | thermomechanically rolled | EN 10149-2 | Flat | ||
300 °C | 10.2 mm²/s Show Material materials with Temperaturleitfähigkeit of 10.2 mm²/s | thermomechanically rolled | EN 10149-2 | Flat | ||
400 °C | 8.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.9 mm²/s | thermomechanically rolled | EN 10149-2 | Flat | ||
500 °C | 7.4 mm²/s Show Material materials with Temperaturleitfähigkeit of 7.4 mm²/s | thermomechanically rolled | EN 10149-2 | Flat | ||
600 °C | 5.8 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.8 mm²/s | thermomechanically rolled | EN 10149-2 | Flat | ||
Wärmeleitfähigkeit | -100 °C | 46.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 46.5 W/(m·K) | thermomechanically rolled | EN 10149-2 | Flat | |
20 °C | 49.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 49.4 W/(m·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
100 °C | 49.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 49.4 W/(m·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
200 °C | 47.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 47.8 W/(m·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
300 °C | 45.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 45.1 W/(m·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
400 °C | 41.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 41.8 W/(m·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
500 °C | 38.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38.6 W/(m·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
600 °C | 35.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 35.3 W/(m·K) | thermomechanically rolled | EN 10149-2 | Flat |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 7 S/m Show Material materials with Elektrische Leitfähigkeit of 7 S/m | Predicted Value | ||||
spezifischer Widerstand | -100 °C | 1.47e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.47e-07 Ω·m | thermomechanically rolled | EN 10149-2 | Flat | |
20 °C | 2.11e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.11e-07 Ω·m | thermomechanically rolled | EN 10149-2 | Flat | ||
100 °C | 2.59e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.59e-07 Ω·m | thermomechanically rolled | EN 10149-2 | Flat | ||
200 °C | 3.3e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.3e-07 Ω·m | thermomechanically rolled | EN 10149-2 | Flat | ||
300 °C | 4.16e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.16e-07 Ω·m | thermomechanically rolled | EN 10149-2 | Flat | ||
400 °C | 5.2e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.2e-07 Ω·m | thermomechanically rolled | EN 10149-2 | Flat | ||
500 °C | 6.41e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.41e-07 Ω·m | thermomechanically rolled | EN 10149-2 | Flat | ||
600 °C | 7.85e-07 Ω·m Show Material materials with spezifischer Widerstand of 7.85e-07 Ω·m | thermomechanically rolled | EN 10149-2 | Flat |
Magnetisch
Property | Value | Comment |
---|---|---|
Curie-Temperatur | 770 °C Show Material materials with Curie-Temperatur of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.015 % Show Material materials with Aluminium of 0.015 % | thermomechanically rolled | EN 10149-2 | Flat |
Kohlenstoff | 0.12 % Show Material materials with Kohlenstoff of 0.12 % | thermomechanically rolled | EN 10149-2 | Flat |
Mangan | 1.6 % Show Material materials with Mangan of 1.6 % | thermomechanically rolled | EN 10149-2 | Flat |
Niobium | 0.09 % Show Material materials with Niobium of 0.09 % | thermomechanically rolled | EN 10149-2 | Flat |
Phosphor | 0.025 % Show Material materials with Phosphor of 0.025 % | thermomechanically rolled | EN 10149-2 | Flat |
Schwefel | 0.015 % Show Material materials with Schwefel of 0.015 % | thermomechanically rolled | EN 10149-2 | Flat |
Silizium | 0.5 % Show Material materials with Silizium of 0.5 % | thermomechanically rolled | EN 10149-2 | Flat |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | thermomechanically rolled | EN 10149-2 | Flat |
Vanadium | 0.2 % Show Material materials with Vanadium of 0.2 % | thermomechanically rolled | EN 10149-2 | Flat |