Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.85 g/cm³ Show Material materials with Dichte of 7.85 g/cm³ | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 17.8 % Show Material materials with Dehnung of 17.8 % | Predicted Value, A200 | ||||
21.5 % Show Material materials with Dehnung of 21.5 % | Predicted Value, A5 | |||||
23.8 % Show Material materials with Dehnung of 23.8 % | Predicted Value, A50 | |||||
20 °C | 13 % Show Material materials with Dehnung of 13 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 14 % Show Material materials with Dehnung of 14 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 15 % Show Material materials with Dehnung of 15 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 15 % Show Material materials with Dehnung of 15 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 16 % Show Material materials with Dehnung of 16 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 16 % Show Material materials with Dehnung of 16 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 17 % Show Material materials with Dehnung of 17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 17 % Show Material materials with Dehnung of 17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 18 % Show Material materials with Dehnung of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 18 % Show Material materials with Dehnung of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 18 % Show Material materials with Dehnung of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 19 % Show Material materials with Dehnung of 19 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 19 % Show Material materials with Dehnung of 19 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 19 % Show Material materials with Dehnung of 19 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 20 % Show Material materials with Dehnung of 20 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 21 % Show Material materials with Dehnung of 21 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 21 % Show Material materials with Dehnung of 21 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 22 % Show Material materials with Dehnung of 22 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 23 % Show Material materials with Dehnung of 23 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Elastizitätsmodul | -100 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 164 GPa Show Material materials with Elastizitätsmodul of 164 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Flächenreduzierung | 43.7 % Show Material materials with Flächenreduzierung of 43.7 % | Predicted Value, Transverse | ||||
50.5 % Show Material materials with Flächenreduzierung of 50.5 % | Predicted Value | |||||
Härte, Brinell | 246 [-] Show Material materials with Härte, Brinell of 246 [-] | Predicted Value, Transverse | ||||
Poissonzahl | 20 °C | 0.284 [-] Show Material materials with Poissonzahl of 0.284 [-] | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
Scherfestigkeit | 487.6 MPa Show Material materials with Scherfestigkeit of 487.6 MPa | Predicted Value | ||||
Schubmodule | 82 GPa Show Material materials with Schubmodule of 82 GPa | Typical for Low Carbon Steel | ||||
Streckgrenze | 248.3 MPa Show Material materials with Streckgrenze of 248.3 MPa | Predicted Value, RP1 | ||||
307.7 MPa Show Material materials with Streckgrenze of 307.7 MPa | Predicted Value, Transverse | |||||
311.8 MPa Show Material materials with Streckgrenze of 311.8 MPa | Predicted Value, RP1 Transverse | |||||
334.3 MPa Show Material materials with Streckgrenze of 334.3 MPa | Predicted Value, RP05 | |||||
348.8 MPa Show Material materials with Streckgrenze of 348.8 MPa | Predicted Value, RP02 | |||||
454.2 MPa Show Material materials with Streckgrenze of 454.2 MPa | Predicted Value, RP02 Transverse | |||||
470 MPa Show Material materials with Streckgrenze of 470 MPa | Predicted Value, RP002 | |||||
20 °C | 205 MPa Show Material materials with Streckgrenze of 205 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 215 MPa Show Material materials with Streckgrenze of 215 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 225 MPa Show Material materials with Streckgrenze of 225 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 235 MPa Show Material materials with Streckgrenze of 235 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 245 MPa Show Material materials with Streckgrenze of 245 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 255 MPa Show Material materials with Streckgrenze of 255 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 265 MPa Show Material materials with Streckgrenze of 265 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 275 MPa Show Material materials with Streckgrenze of 275 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 180 - 220 MPa Show Material materials with Streckgrenze of 180 - 220 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 180 - 210 MPa Show Material materials with Streckgrenze of 180 - 210 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 180 - 188 MPa Show Material materials with Streckgrenze of 180 - 188 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 180 MPa Show Material materials with Streckgrenze of 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 188 - 220 MPa Show Material materials with Streckgrenze of 188 - 220 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 188 - 210 MPa Show Material materials with Streckgrenze of 188 - 210 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 188 MPa Show Material materials with Streckgrenze of 188 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 210 - 220 MPa Show Material materials with Streckgrenze of 210 - 220 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 210 MPa Show Material materials with Streckgrenze of 210 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 220 MPa Show Material materials with Streckgrenze of 220 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 155 - 190 MPa Show Material materials with Streckgrenze of 155 - 190 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 155 - 180 MPa Show Material materials with Streckgrenze of 155 - 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 155 - 162 MPa Show Material materials with Streckgrenze of 155 - 162 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 155 MPa Show Material materials with Streckgrenze of 155 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 162 - 190 MPa Show Material materials with Streckgrenze of 162 - 190 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 162 - 180 MPa Show Material materials with Streckgrenze of 162 - 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 162 MPa Show Material materials with Streckgrenze of 162 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 180 MPa Show Material materials with Streckgrenze of 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 180 - 190 MPa Show Material materials with Streckgrenze of 180 - 190 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 190 MPa Show Material materials with Streckgrenze of 190 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 144 - 180 MPa Show Material materials with Streckgrenze of 144 - 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 144 - 170 MPa Show Material materials with Streckgrenze of 144 - 170 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 144 - 150 MPa Show Material materials with Streckgrenze of 144 - 150 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 144 MPa Show Material materials with Streckgrenze of 144 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 150 - 180 MPa Show Material materials with Streckgrenze of 150 - 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 150 - 170 MPa Show Material materials with Streckgrenze of 150 - 170 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 150 MPa Show Material materials with Streckgrenze of 150 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 170 - 180 MPa Show Material materials with Streckgrenze of 170 - 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 170 MPa Show Material materials with Streckgrenze of 170 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 180 MPa Show Material materials with Streckgrenze of 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 119 - 150 MPa Show Material materials with Streckgrenze of 119 - 150 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 119 - 140 MPa Show Material materials with Streckgrenze of 119 - 140 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 119 - 124 MPa Show Material materials with Streckgrenze of 119 - 124 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 119 MPa Show Material materials with Streckgrenze of 119 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 124 - 150 MPa Show Material materials with Streckgrenze of 124 - 150 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 124 - 140 MPa Show Material materials with Streckgrenze of 124 - 140 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 124 MPa Show Material materials with Streckgrenze of 124 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 140 - 150 MPa Show Material materials with Streckgrenze of 140 - 150 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 140 MPa Show Material materials with Streckgrenze of 140 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 150 MPa Show Material materials with Streckgrenze of 150 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
Zugfestigkeit | 20 °C | 380 - 580 MPa Show Material materials with Zugfestigkeit of 380 - 580 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 380 - 560 MPa Show Material materials with Zugfestigkeit of 380 - 560 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 380 - 540 MPa Show Material materials with Zugfestigkeit of 380 - 540 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 400 - 580 MPa Show Material materials with Zugfestigkeit of 400 - 580 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 400 - 560 MPa Show Material materials with Zugfestigkeit of 400 - 560 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 400 - 540 MPa Show Material materials with Zugfestigkeit of 400 - 540 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 410 - 580 MPa Show Material materials with Zugfestigkeit of 410 - 580 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 410 - 560 MPa Show Material materials with Zugfestigkeit of 410 - 560 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 410 - 540 MPa Show Material materials with Zugfestigkeit of 410 - 540 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 430 - 580 MPa Show Material materials with Zugfestigkeit of 430 - 580 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 430 - 560 MPa Show Material materials with Zugfestigkeit of 430 - 560 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 430 - 540 MPa Show Material materials with Zugfestigkeit of 430 - 540 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.08e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 1.19e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 1.25e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 1.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 1.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 1.45e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 1.49e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Max. Betriebstemperatur | 336.1 °C Show Material materials with Max. Betriebstemperatur of 336.1 °C | Predicted Value, Long | ||||
500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | Typical for Carbon Steel | |||||
Schmelzpunkt | 1480 - 1526 °C Show Material materials with Schmelzpunkt of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Spezifische Wärmekapazität | -100 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 558 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 587 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Temperaturleitfähigkeit | 20 °C | 14.8 mm²/s Show Material materials with Temperaturleitfähigkeit of 14.8 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
100 °C | 13.6 mm²/s Show Material materials with Temperaturleitfähigkeit of 13.6 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 12.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 12.1 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 10.6 mm²/s Show Material materials with Temperaturleitfähigkeit of 10.6 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 9.2 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.2 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 7.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 7.7 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 6.2 mm²/s Show Material materials with Temperaturleitfähigkeit of 6.2 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Wärmeleitfähigkeit | 20 °C | 53.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 53.4 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
100 °C | 52.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 52.9 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 50.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 50.3 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 46.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 46.7 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 43.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 43.3 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 39.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39.8 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 36.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36.7 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 8 S/m Show Material materials with Elektrische Leitfähigkeit of 8 S/m | Predicted Value | ||||
spezifischer Widerstand | 20 °C | 1.95e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.95e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
100 °C | 2.42e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.42e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 3.14e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.14e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 4.02e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.02e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 5.02e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.02e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 6.21e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.21e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 7.55e-07 Ω·m Show Material materials with spezifischer Widerstand of 7.55e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Magnetisch
Property | Value | Comment |
---|---|---|
Curie-Temperatur | 770 °C Show Material materials with Curie-Temperatur of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Kohlenstoff | 0.21 % Show Material materials with Kohlenstoff of 0.21 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Kupfer | 0.55 % Show Material materials with Kupfer of 0.55 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Mangan | 1.5 % Show Material materials with Mangan of 1.5 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Phosphor | 0.035 % Show Material materials with Phosphor of 0.035 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Schwefel | 0.035 % Show Material materials with Schwefel of 0.035 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Stickstoff | 0.012 % Show Material materials with Stickstoff of 0.012 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |