DIN 1725-1 Grade 3.3547 H18

View suppliers (11)
Want to keep this datasheet? Save it now in your required format

Description

The alloy AlMg4,5Mn belongs to the nature-hard aluminum wrought materials, so a strength increase can be achieved only by cold forming, not by a purposeful heat treatment. The material is characterised by good corrosion resistance. It is sea water steady and steady against saline atmosphere. Increasing Mg+Mn content makes the extrusion more difficult, but strength and very low-temperature behaviour improve. The alloy is well weldable. Even in the welding seams strength lie within the range of AlMg5. The alloy AlMg4Mn is standardised as semi-finished material only as sheet metal or strips, thickness: >= 0,35 mm (DIN 1745). Application: rolling shutter and roll gates (sheet metal profiles), in the apparatus engineering for tank bottoms, very low-temperature tanks, heat exchangers and pipings. In the construction of vehicles for superstructures as well as tank and silo trucks, dump truck hollows, buses, bumpers, car body and safety-related parts. In shipbuilding for trunk, superstructures, sail masts and radar equipment

Related Standards

Equivalent Materials

Diese Materialdaten wurden von WIAM,AluKey zur Verfügung gestellt

Alle Daten beziehen sich auf Raumtemperatur soweit nicht anderweitig spezifiziert. SI Einheiten werden verwendt soweit nicht anderweitig spezifiziert.
Äquivalente Standards sind ähnlich zu einem oder mehreren Standards die der Anbieter angegeben hat. Manche äquivalente Standards können strikter sein oder außerhalb der Bedingungen des ursprünglichen Standards.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Eigenschaften

Allgemein

PropertyTemperatureValueConditionRelated Standards

Dichte

2.66 g/cm³

Show Material materials with Dichte of 2.66 g/cm³

H18

EN 573-3, EN 1592

20.0 °C

2.66 g/cm³

Show Material materials with Dichte of 2.66 g/cm³

H18

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Mechanisch

PropertyTemperatureValueConditionRelated StandardsComment

Elastizitätsmodul

71.0 GPa

Show Material materials with Elastizitätsmodul of 71.0 GPa

H18

EN 573-3, EN 1592

20.0 °C

72.0 GPa

Show Material materials with Elastizitätsmodul of 72.0 GPa

H18

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poissonzahl

0.33 [-]

Show Material materials with Poissonzahl of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Schubmodule

26.8 GPa

Show Material materials with Schubmodule of 26.8 GPa

H18

EN 573-3, EN 1592

20.0 °C

27.0 GPa

Show Material materials with Schubmodule of 27.0 GPa

H18

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Zugfestigkeit

-196.0 °C

575.0 MPa

Show Material materials with Zugfestigkeit of 575.0 MPa

H18

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

420.0 MPa

Show Material materials with Zugfestigkeit of 420.0 MPa

H18

EN 573-3, EN 1592

20.0 °C

445.0 MPa

Show Material materials with Zugfestigkeit of 445.0 MPa

H18

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Thermisch

PropertyTemperatureValueConditionRelated StandardsComment

Koeffizient der thermischen Ausdehnung

-50 °C

2.23e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.23e-05 1/K

H18

EN 573-3, EN 1592, DIN 1725-1, EN 573-4, VdTÜV WB 255

-50.0 °C

2.23e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.23e-05 1/K

H18

EN 573-3, EN 1592, DIN 1725-1, EN 573-4, VdTÜV WB 255

20 °C

2.23e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.23e-05 1/K

H18

EN 573-3, EN 1592, DIN 1725-1, EN 573-4, VdTÜV WB 255

20 °C

2.42e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.42e-05 1/K

H18

EN 573-3, EN 1592, DIN 1725-1, EN 573-4, VdTÜV WB 255

20 °C

2.4999999999999998e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4999999999999998e-05 1/K

H18

EN 573-3, EN 1592

20 °C

2.6e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.6e-05 1/K

H18

EN 573-3, EN 1592, DIN 1725-1, EN 573-4, VdTÜV WB 255

100 °C

2.42e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.42e-05 1/K

H18

EN 573-3, EN 1592, DIN 1725-1, EN 573-4, VdTÜV WB 255

100.0 °C

2.42e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.42e-05 1/K

H18

EN 573-3, EN 1592, DIN 1725-1, EN 573-4, VdTÜV WB 255

200 °C

2.4999999999999998e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4999999999999998e-05 1/K

H18

EN 573-3, EN 1592

200.0 °C

2.5e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5e-05 1/K

H18

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

300 °C

2.6e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.6e-05 1/K

H18

EN 573-3, EN 1592, DIN 1725-1, EN 573-4, VdTÜV WB 255

300.0 °C

2.6e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.6e-05 1/K

H18

EN 573-3, EN 1592, DIN 1725-1, EN 573-4, VdTÜV WB 255

Max. Betriebstemperatur

-195.0 - 50.0 °C

Show Material materials with Max. Betriebstemperatur of -195.0 - 50.0 °C

H18

DIN 1725-1, EN 573-3, EN 573-4

Long

150.0 °C

Show Material materials with Max. Betriebstemperatur of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Schmelzpunkt

574.0 - 638.0 °C

Show Material materials with Schmelzpunkt of 574.0 - 638.0 °C

H18

EN 573-3, EN 1592

Spezifische Wärmekapazität

900.0 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K)

H18

EN 573-3, EN 1592

20.0 °C

900.0 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K)

H18

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

Wärmeleitfähigkeit

20.0 °C

110.0 - 140.0 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 110.0 - 140.0 W/(m·K)

H18

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 1592

Elektrisch

PropertyTemperatureValueConditionRelated Standards

Elektrische Leitfähigkeit

20.0 °C

16000000.0 - 19000000.0 S/m

Show Material materials with Elektrische Leitfähigkeit of 16000000.0 - 19000000.0 S/m

H18

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 1592

spezifischer Widerstand

5.26e-08 - 6.25e-08 Ω·m

Show Material materials with spezifischer Widerstand of 5.26e-08 - 6.25e-08 Ω·m

H18

EN 573-3, EN 1592

Chemical properties

PropertyValueConditionRelated Standards

Chrom

0.05 - 0.25 %

Show Material materials with Chrom of 0.05 - 0.25 %

H18

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 1592

Eisen

0.4 %

Show Material materials with Eisen of 0.4 %

H18

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255

0.40 %

Show Material materials with Eisen of 0.40 %

H18

EN 573-3, EN 1592

Kupfer

0.1 %

Show Material materials with Kupfer of 0.1 %

H18

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 1592

Magnesium

4.0 - 4.9 %

Show Material materials with Magnesium of 4.0 - 4.9 %

H18

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 1592

Mangan

0.4 - 1.0 %

Show Material materials with Mangan of 0.4 - 1.0 %

H18

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 1592

Silizium

0.4 %

Show Material materials with Silizium of 0.4 %

H18

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 1592

Titan

0.15 %

Show Material materials with Titan of 0.15 %

H18

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 1592

Zink

0.25 %

Show Material materials with Zink of 0.25 %

H18

DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 255, EN 1592

Technological properties

Property
Anodizing

decorative: sufficient, Protective: good

Brazing

hard brazing (with flux/ without flux): poor / poor, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Seawater: very good, weathering: very good

Workability

Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (O)