Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.848 - 7.85 g/cm³ Show Material materials with Dichte of 7.848 - 7.85 g/cm³ | normalized and tempered (+NT) | EN 10028-2 | Flat |
20 °C | 7.848 g/cm³ Show Material materials with Dichte of 7.848 g/cm³ | normalized and tempered (+NT) | EN 10028-2 | Flat | |
20 °C | 7.85 g/cm³ Show Material materials with Dichte of 7.85 g/cm³ | normalized and tempered (+NT) | EN 10028-2 | Flat | |
50 °C | 7.839 g/cm³ Show Material materials with Dichte of 7.839 g/cm³ | normalized and tempered (+NT) | EN 10028-2 | Flat | |
100 °C | 7.824 g/cm³ Show Material materials with Dichte of 7.824 g/cm³ | normalized and tempered (+NT) | EN 10028-2 | Flat | |
150 °C | 7.809 g/cm³ Show Material materials with Dichte of 7.809 g/cm³ | normalized and tempered (+NT) | EN 10028-2 | Flat | |
200 °C | 7.792 g/cm³ Show Material materials with Dichte of 7.792 g/cm³ | normalized and tempered (+NT) | EN 10028-2 | Flat | |
250 °C | 7.774 g/cm³ Show Material materials with Dichte of 7.774 g/cm³ | normalized and tempered (+NT) | EN 10028-2 | Flat | |
300 °C | 7.756 g/cm³ Show Material materials with Dichte of 7.756 g/cm³ | normalized and tempered (+NT) | EN 10028-2 | Flat | |
350 °C | 7.738 g/cm³ Show Material materials with Dichte of 7.738 g/cm³ | normalized and tempered (+NT) | EN 10028-2 | Flat | |
400 °C | 7.719 g/cm³ Show Material materials with Dichte of 7.719 g/cm³ | normalized and tempered (+NT) | EN 10028-2 | Flat | |
450 °C | 7.7 g/cm³ Show Material materials with Dichte of 7.7 g/cm³ | normalized and tempered (+NT) | EN 10028-2 | Flat | |
500 °C | 7.681 g/cm³ Show Material materials with Dichte of 7.681 g/cm³ | normalized and tempered (+NT) | EN 10028-2 | Flat | |
550 °C | 7.662 g/cm³ Show Material materials with Dichte of 7.662 g/cm³ | normalized and tempered (+NT) | EN 10028-2 | Flat | |
600 °C | 7.643 g/cm³ Show Material materials with Dichte of 7.643 g/cm³ | normalized and tempered (+NT) | EN 10028-2 | Flat |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 16.5 % Show Material materials with Dehnung of 16.5 % | Predicted Value, A80 Transverse | ||||
17.6 % Show Material materials with Dehnung of 17.6 % | Predicted Value, A80 | |||||
18.0 % Show Material materials with Dehnung of 18.0 % | Predicted Value, A200 | |||||
20.2 % Show Material materials with Dehnung of 20.2 % | Predicted Value, A5 | |||||
22.1 % Show Material materials with Dehnung of 22.1 % | Predicted Value, A50 | |||||
20 °C | 19 % Show Material materials with Dehnung of 19 % | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 19 % Show Material materials with Dehnung of 19 % | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
Elastizitätsmodul | -100 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | |
20 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 212 - 212.5 GPa Show Material materials with Elastizitätsmodul of 212 - 212.5 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 212.5 GPa Show Material materials with Elastizitätsmodul of 212.5 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
50 °C | 211.6 GPa Show Material materials with Elastizitätsmodul of 211.6 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 207 - 209 GPa Show Material materials with Elastizitätsmodul of 207 - 209 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 207 - 208.9 GPa Show Material materials with Elastizitätsmodul of 207 - 208.9 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 208.9 - 209 GPa Show Material materials with Elastizitätsmodul of 208.9 - 209 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 208.9 GPa Show Material materials with Elastizitätsmodul of 208.9 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 209 GPa Show Material materials with Elastizitätsmodul of 209 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
150 °C | 205.5 GPa Show Material materials with Elastizitätsmodul of 205.5 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 199 - 202 GPa Show Material materials with Elastizitätsmodul of 199 - 202 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 199 - 201.8 GPa Show Material materials with Elastizitätsmodul of 199 - 201.8 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 201.8 - 202 GPa Show Material materials with Elastizitätsmodul of 201.8 - 202 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 201.8 GPa Show Material materials with Elastizitätsmodul of 201.8 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 202 GPa Show Material materials with Elastizitätsmodul of 202 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
250 °C | 197.7 GPa Show Material materials with Elastizitätsmodul of 197.7 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 192 - 193 GPa Show Material materials with Elastizitätsmodul of 192 - 193 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 192 - 193.4 GPa Show Material materials with Elastizitätsmodul of 192 - 193.4 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 193 GPa Show Material materials with Elastizitätsmodul of 193 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 193 - 193.4 GPa Show Material materials with Elastizitätsmodul of 193 - 193.4 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 193.4 GPa Show Material materials with Elastizitätsmodul of 193.4 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
350 °C | 189.2 GPa Show Material materials with Elastizitätsmodul of 189.2 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 184 - 185 GPa Show Material materials with Elastizitätsmodul of 184 - 185 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 184 - 184.8 GPa Show Material materials with Elastizitätsmodul of 184 - 184.8 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 184.8 - 185 GPa Show Material materials with Elastizitätsmodul of 184.8 - 185 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 184.8 GPa Show Material materials with Elastizitätsmodul of 184.8 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 185 GPa Show Material materials with Elastizitätsmodul of 185 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
450 °C | 180.4 GPa Show Material materials with Elastizitätsmodul of 180.4 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 175 - 176 GPa Show Material materials with Elastizitätsmodul of 175 - 176 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 175 - 175.9 GPa Show Material materials with Elastizitätsmodul of 175 - 175.9 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 175.9 - 176 GPa Show Material materials with Elastizitätsmodul of 175.9 - 176 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 175.9 GPa Show Material materials with Elastizitätsmodul of 175.9 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 176 GPa Show Material materials with Elastizitätsmodul of 176 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
550 °C | 171.3 GPa Show Material materials with Elastizitätsmodul of 171.3 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 164 - 166 GPa Show Material materials with Elastizitätsmodul of 164 - 166 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 164 GPa Show Material materials with Elastizitätsmodul of 164 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 164 - 166.6 GPa Show Material materials with Elastizitätsmodul of 164 - 166.6 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 166 GPa Show Material materials with Elastizitätsmodul of 166 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 166 - 166.6 GPa Show Material materials with Elastizitätsmodul of 166 - 166.6 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 166.6 GPa Show Material materials with Elastizitätsmodul of 166.6 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
Flächenreduzierung | 43.4 % Show Material materials with Flächenreduzierung of 43.4 % | Predicted Value | ||||
43.9 % Show Material materials with Flächenreduzierung of 43.9 % | Predicted Value, Transverse | |||||
Härte, Brinell | 224 [-] Show Material materials with Härte, Brinell of 224 [-] | Predicted Value, Transverse | ||||
Poissonzahl | 20 °C | 0.283 [-] Show Material materials with Poissonzahl of 0.283 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | |
20 °C | 0.284 [-] Show Material materials with Poissonzahl of 0.284 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
50 °C | 0.284 [-] Show Material materials with Poissonzahl of 0.284 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 0.283 [-] Show Material materials with Poissonzahl of 0.283 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
150 °C | 0.285 [-] Show Material materials with Poissonzahl of 0.285 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 0.287 [-] Show Material materials with Poissonzahl of 0.287 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
250 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 0.292 [-] Show Material materials with Poissonzahl of 0.292 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
350 °C | 0.295 [-] Show Material materials with Poissonzahl of 0.295 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 0.296 [-] Show Material materials with Poissonzahl of 0.296 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
450 °C | 0.299 [-] Show Material materials with Poissonzahl of 0.299 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 0.301 [-] Show Material materials with Poissonzahl of 0.301 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
550 °C | 0.305 [-] Show Material materials with Poissonzahl of 0.305 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 0.31 [-] Show Material materials with Poissonzahl of 0.31 [-] | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
Scherfestigkeit | 602.2 MPa Show Material materials with Scherfestigkeit of 602.2 MPa | Predicted Value | ||||
Schubmodule | 20 °C | 82.8 GPa Show Material materials with Schubmodule of 82.8 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | |
50 °C | 82.4 GPa Show Material materials with Schubmodule of 82.4 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 81.4 GPa Show Material materials with Schubmodule of 81.4 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
150 °C | 80.0 GPa Show Material materials with Schubmodule of 80.0 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 78.4 GPa Show Material materials with Schubmodule of 78.4 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
250 °C | 76.6 GPa Show Material materials with Schubmodule of 76.6 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 74.8 GPa Show Material materials with Schubmodule of 74.8 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
350 °C | 73.1 GPa Show Material materials with Schubmodule of 73.1 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 71.3 GPa Show Material materials with Schubmodule of 71.3 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
450 °C | 69.5 GPa Show Material materials with Schubmodule of 69.5 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 67.6 GPa Show Material materials with Schubmodule of 67.6 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
550 °C | 65.6 GPa Show Material materials with Schubmodule of 65.6 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 63.6 GPa Show Material materials with Schubmodule of 63.6 GPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
Streckgrenze | 256 MPa Show Material materials with Streckgrenze of 256 MPa | Predicted Value, RP1 | ||||
265.2 MPa Show Material materials with Streckgrenze of 265.2 MPa | Predicted Value, RP1 Transverse | |||||
367.8 MPa Show Material materials with Streckgrenze of 367.8 MPa | Predicted Value, RP05 | |||||
368.9 MPa Show Material materials with Streckgrenze of 368.9 MPa | Predicted Value, RP02 Transverse | |||||
481.7 MPa Show Material materials with Streckgrenze of 481.7 MPa | Predicted Value, RP002 | |||||
20 °C | 255 MPa Show Material materials with Streckgrenze of 255 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 255 MPa Show Material materials with Streckgrenze of 255 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 270 MPa Show Material materials with Streckgrenze of 270 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 270 MPa Show Material materials with Streckgrenze of 270 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 290 MPa Show Material materials with Streckgrenze of 290 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 290 MPa Show Material materials with Streckgrenze of 290 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 300 MPa Show Material materials with Streckgrenze of 300 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 300 MPa Show Material materials with Streckgrenze of 300 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
50 °C | 250 MPa Show Material materials with Streckgrenze of 250 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
50 °C | 265 MPa Show Material materials with Streckgrenze of 265 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
50 °C | 285 MPa Show Material materials with Streckgrenze of 285 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
50 °C | 294 MPa Show Material materials with Streckgrenze of 294 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
100 °C | 242 MPa Show Material materials with Streckgrenze of 242 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
100 °C | 256 MPa Show Material materials with Streckgrenze of 256 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
100 °C | 275 MPa Show Material materials with Streckgrenze of 275 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
100 °C | 285 MPa Show Material materials with Streckgrenze of 285 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
150 °C | 229 MPa Show Material materials with Streckgrenze of 229 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
150 °C | 242 MPa Show Material materials with Streckgrenze of 242 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
150 °C | 260 MPa Show Material materials with Streckgrenze of 260 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
150 °C | 269 MPa Show Material materials with Streckgrenze of 269 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
200 °C | 214 MPa Show Material materials with Streckgrenze of 214 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
200 °C | 227 MPa Show Material materials with Streckgrenze of 227 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
200 °C | 243 MPa Show Material materials with Streckgrenze of 243 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
200 °C | 252 MPa Show Material materials with Streckgrenze of 252 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
250 °C | 199 MPa Show Material materials with Streckgrenze of 199 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
250 °C | 210 MPa Show Material materials with Streckgrenze of 210 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
250 °C | 226 MPa Show Material materials with Streckgrenze of 226 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
250 °C | 234 MPa Show Material materials with Streckgrenze of 234 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
300 °C | 184 MPa Show Material materials with Streckgrenze of 184 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
300 °C | 195 MPa Show Material materials with Streckgrenze of 195 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
300 °C | 209 MPa Show Material materials with Streckgrenze of 209 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
300 °C | 216 MPa Show Material materials with Streckgrenze of 216 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
350 °C | 170 MPa Show Material materials with Streckgrenze of 170 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
350 °C | 180 MPa Show Material materials with Streckgrenze of 180 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
350 °C | 194 MPa Show Material materials with Streckgrenze of 194 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
350 °C | 200 MPa Show Material materials with Streckgrenze of 200 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
400 °C | 159 MPa Show Material materials with Streckgrenze of 159 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
400 °C | 168 MPa Show Material materials with Streckgrenze of 168 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
400 °C | 180 MPa Show Material materials with Streckgrenze of 180 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
400 °C | 186 MPa Show Material materials with Streckgrenze of 186 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
450 °C | 148 MPa Show Material materials with Streckgrenze of 148 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
450 °C | 157 MPa Show Material materials with Streckgrenze of 157 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
450 °C | 169 MPa Show Material materials with Streckgrenze of 169 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
450 °C | 175 MPa Show Material materials with Streckgrenze of 175 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
500 °C | 139 MPa Show Material materials with Streckgrenze of 139 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
500 °C | 148 MPa Show Material materials with Streckgrenze of 148 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
500 °C | 159 MPa Show Material materials with Streckgrenze of 159 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
500 °C | 164 MPa Show Material materials with Streckgrenze of 164 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | RP02 | |
Zugfestigkeit | 20 °C | 430 - 600 MPa Show Material materials with Zugfestigkeit of 430 - 600 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse |
20 °C | 430 - 590 MPa Show Material materials with Zugfestigkeit of 430 - 590 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 430 - 580 MPa Show Material materials with Zugfestigkeit of 430 - 580 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 430 - 600 MPa Show Material materials with Zugfestigkeit of 430 - 600 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 430 - 590 MPa Show Material materials with Zugfestigkeit of 430 - 590 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 430 - 580 MPa Show Material materials with Zugfestigkeit of 430 - 580 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 440 - 600 MPa Show Material materials with Zugfestigkeit of 440 - 600 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 440 - 590 MPa Show Material materials with Zugfestigkeit of 440 - 590 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 440 - 580 MPa Show Material materials with Zugfestigkeit of 440 - 580 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 440 - 600 MPa Show Material materials with Zugfestigkeit of 440 - 600 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 440 - 590 MPa Show Material materials with Zugfestigkeit of 440 - 590 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 440 - 580 MPa Show Material materials with Zugfestigkeit of 440 - 580 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 450 - 600 MPa Show Material materials with Zugfestigkeit of 450 - 600 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 450 - 590 MPa Show Material materials with Zugfestigkeit of 450 - 590 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 450 - 580 MPa Show Material materials with Zugfestigkeit of 450 - 580 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | Transverse | |
20 °C | 450 - 600 MPa Show Material materials with Zugfestigkeit of 450 - 600 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 450 - 590 MPa Show Material materials with Zugfestigkeit of 450 - 590 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 450 - 580 MPa Show Material materials with Zugfestigkeit of 450 - 580 MPa | normalized and tempered (+NT) | EN 10028-2 | Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.05e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | |
20 °C | 1.15e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.15e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 1.21e-05 - 1.22e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 - 1.22e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 1.21e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 1.22e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.22e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 1.27e-05 - 1.29e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27e-05 - 1.29e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 1.27e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 1.29e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.29e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 1.32e-05 - 1.34e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 - 1.34e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 1.32e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 1.34e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.34e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 1.36e-05 - 1.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 - 1.4e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 1.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 1.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 1.4e-05 - 1.43e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-05 - 1.43e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 1.43e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.43e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 1.44e-05 - 1.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.44e-05 - 1.46e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 1.44e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.44e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 1.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.46e-05 1/K | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
Max. Betriebstemperatur | 400 - 550 °C Show Material materials with Max. Betriebstemperatur of 400 - 550 °C | normalized and tempered (+NT) | EN 10028-2 | Flat | Long | |
Schmelzpunkt | 1382 - 1529 °C Show Material materials with Schmelzpunkt of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | ||||
Spezifische Wärmekapazität | -100 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | |
20 °C | 430 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 430 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 430 - 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 430 - 461 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 479 - 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 - 500 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 500 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 499 - 540 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 - 540 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 540 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 540 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 517 - 580 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 - 580 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 580 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 580 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 536 - 620 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 - 620 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 620 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 620 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 558 - 690 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 - 690 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 690 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 690 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 587 - 780 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 - 780 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 780 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 780 J/(kg·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
Temperaturleitfähigkeit | 20 °C | 12.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 12.7 mm²/s | normalized and tempered (+NT) | EN 10028-2 | Flat | |
100 °C | 12 mm²/s Show Material materials with Temperaturleitfähigkeit of 12 mm²/s | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 11 mm²/s Show Material materials with Temperaturleitfähigkeit of 11 mm²/s | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 9.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.9 mm²/s | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 8.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.7 mm²/s | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 7.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 7.3 mm²/s | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 6 mm²/s Show Material materials with Temperaturleitfähigkeit of 6 mm²/s | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
Wärmeleitfähigkeit | 20 °C | 45.9 - 46 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 45.9 - 46 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | |
20 °C | 45.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 45.9 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 46 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 46 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 46 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 46 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 46 - 46.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 46 - 46.4 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 46.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 46.4 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 45.6 - 46 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 45.6 - 46 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 45.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 45.6 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 46 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 46 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 43 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 43 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 43 - 43.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 43 - 43.5 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 43.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 43.5 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 40.9 - 41 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 40.9 - 41 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 40.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 40.9 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 41 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 41 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 38 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 38 - 38.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38 - 38.2 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 38.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38.2 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 35.5 - 36 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 35.5 - 36 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 35.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 35.5 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 36 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36 W/(m·K) | normalized and tempered (+NT) | EN 10028-2 | Flat |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 4 S/m Show Material materials with Elektrische Leitfähigkeit of 4 S/m | Predicted Value | ||||
spezifischer Widerstand | 20 °C | 2.27e-07 - 2.3e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.27e-07 - 2.3e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | |
20 °C | 2.27e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.27e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 2.27e-07 - 2.37e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.27e-07 - 2.37e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 2.3e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.3e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 2.3e-07 - 2.37e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.3e-07 - 2.37e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
20 °C | 2.37e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.37e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
50 °C | 2.56e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.56e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 2.76e-07 - 2.8e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.76e-07 - 2.8e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 2.76e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.76e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 2.76e-07 - 2.88e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.76e-07 - 2.88e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 2.8e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.8e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 2.8e-07 - 2.88e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.8e-07 - 2.88e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
100 °C | 2.88e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.88e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
150 °C | 3.21e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.21e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 3.46e-07 - 3.5e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.46e-07 - 3.5e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 3.46e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.46e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 3.46e-07 - 3.59e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.46e-07 - 3.59e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 3.5e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.5e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 3.5e-07 - 3.59e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.5e-07 - 3.59e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
200 °C | 3.59e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.59e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
250 °C | 4.01e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.01e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 4.3e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.3e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 4.3e-07 - 4.31e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.3e-07 - 4.31e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 4.3e-07 - 4.45e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.3e-07 - 4.45e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 4.31e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.31e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 4.31e-07 - 4.45e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.31e-07 - 4.45e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
300 °C | 4.45e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.45e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
350 °C | 4.95e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.95e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 5.3e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.3e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 5.3e-07 - 5.32e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.3e-07 - 5.32e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 5.3e-07 - 5.48e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.3e-07 - 5.48e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 5.32e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.32e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 5.32e-07 - 5.48e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.32e-07 - 5.48e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
400 °C | 5.48e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.48e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
450 °C | 6.06e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.06e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 6.48e-07 - 6.5e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.48e-07 - 6.5e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 6.48e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.48e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 6.48e-07 - 6.63e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.48e-07 - 6.63e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 6.5e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.5e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 6.5e-07 - 6.63e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.5e-07 - 6.63e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
500 °C | 6.63e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.63e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
550 °C | 7.28e-07 Ω·m Show Material materials with spezifischer Widerstand of 7.28e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 7.8e-07 Ω·m Show Material materials with spezifischer Widerstand of 7.8e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 7.8e-07 - 7.81e-07 Ω·m Show Material materials with spezifischer Widerstand of 7.8e-07 - 7.81e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 7.8e-07 - 7.97e-07 Ω·m Show Material materials with spezifischer Widerstand of 7.8e-07 - 7.97e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 7.81e-07 Ω·m Show Material materials with spezifischer Widerstand of 7.81e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 7.81e-07 - 7.97e-07 Ω·m Show Material materials with spezifischer Widerstand of 7.81e-07 - 7.97e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat | ||
600 °C | 7.97e-07 Ω·m Show Material materials with spezifischer Widerstand of 7.97e-07 Ω·m | normalized and tempered (+NT) | EN 10028-2 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.7 - 1.15 % Show Material materials with Chrom of 0.7 - 1.15 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Kohlenstoff | 0.08 - 0.18 % Show Material materials with Kohlenstoff of 0.08 - 0.18 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Kupfer | 0.3 % Show Material materials with Kupfer of 0.3 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Mangan | 0.4 - 1 % Show Material materials with Mangan of 0.4 - 1 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Molybdän | 0.4 - 0.6 % Show Material materials with Molybdän of 0.4 - 0.6 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Phosphor | 0.025 % Show Material materials with Phosphor of 0.025 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Schwefel | 0.01 % Show Material materials with Schwefel of 0.01 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Silizium | 0.35 % Show Material materials with Silizium of 0.35 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Stickstoff | 0.012 % Show Material materials with Stickstoff of 0.012 % | normalized and tempered (+NT) | EN 10028-2 | Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |