Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.8 g/cm³ Show Material materials with Dichte of 7.8 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat |
20 °C | 7.8 - 7.85 g/cm³ Show Material materials with Dichte of 7.8 - 7.85 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 7.85 g/cm³ Show Material materials with Dichte of 7.85 g/cm³ | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 15.4 % Show Material materials with Dehnung of 15.4 % | Predicted Value, A200 | ||||
15.8 % Show Material materials with Dehnung of 15.8 % | Predicted Value, A80 | |||||
17.3 % Show Material materials with Dehnung of 17.3 % | Predicted Value, A80 Transverse | |||||
18.7 % Show Material materials with Dehnung of 18.7 % | Predicted Value, A5 | |||||
19.5 % Show Material materials with Dehnung of 19.5 % | Predicted Value, A50 | |||||
20 °C | 22 % Show Material materials with Dehnung of 22 % | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 22 % Show Material materials with Dehnung of 22 % | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Elastizitätsmodul | -100 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 210 GPa Show Material materials with Elastizitätsmodul of 210 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 210 - 212 GPa Show Material materials with Elastizitätsmodul of 210 - 212 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 205 GPa Show Material materials with Elastizitätsmodul of 205 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 205 - 207 GPa Show Material materials with Elastizitätsmodul of 205 - 207 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 195 GPa Show Material materials with Elastizitätsmodul of 195 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 195 - 199 GPa Show Material materials with Elastizitätsmodul of 195 - 199 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 185 GPa Show Material materials with Elastizitätsmodul of 185 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 185 - 192 GPa Show Material materials with Elastizitätsmodul of 185 - 192 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 175 - 184 GPa Show Material materials with Elastizitätsmodul of 175 - 184 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 164 GPa Show Material materials with Elastizitätsmodul of 164 GPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Flächenreduzierung | 40.9 % Show Material materials with Flächenreduzierung of 40.9 % | Predicted Value | ||||
43.4 % Show Material materials with Flächenreduzierung of 43.4 % | Predicted Value, Transverse | |||||
Härte, Brinell | 243 [-] Show Material materials with Härte, Brinell of 243 [-] | Predicted Value, Transverse | ||||
Poissonzahl | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Low Carbon Steel | ||||
Scherfestigkeit | 539.5 MPa Show Material materials with Scherfestigkeit of 539.5 MPa | Predicted Value | ||||
Schubmodule | 82 GPa Show Material materials with Schubmodule of 82 GPa | Typical for Low Carbon Steel | ||||
Streckgrenze | 288.8 MPa Show Material materials with Streckgrenze of 288.8 MPa | Predicted Value, RP1 Transverse | ||||
295.5 MPa Show Material materials with Streckgrenze of 295.5 MPa | Predicted Value, RP1 | |||||
372.9 MPa Show Material materials with Streckgrenze of 372.9 MPa | Predicted Value, RP05 | |||||
398.7 MPa Show Material materials with Streckgrenze of 398.7 MPa | Predicted Value, RP02 Transverse | |||||
601.7 MPa Show Material materials with Streckgrenze of 601.7 MPa | Predicted Value, RP002 | |||||
20 °C | 185 MPa Show Material materials with Streckgrenze of 185 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 185 MPa Show Material materials with Streckgrenze of 185 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 200 MPa Show Material materials with Streckgrenze of 200 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 200 MPa Show Material materials with Streckgrenze of 200 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 215 MPa Show Material materials with Streckgrenze of 215 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 215 MPa Show Material materials with Streckgrenze of 215 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 245 MPa Show Material materials with Streckgrenze of 245 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 245 MPa Show Material materials with Streckgrenze of 245 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 255 MPa Show Material materials with Streckgrenze of 255 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 255 MPa Show Material materials with Streckgrenze of 255 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 265 MPa Show Material materials with Streckgrenze of 265 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 265 MPa Show Material materials with Streckgrenze of 265 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
50 °C | 179 MPa Show Material materials with Streckgrenze of 179 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 193 MPa Show Material materials with Streckgrenze of 193 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 208 MPa Show Material materials with Streckgrenze of 208 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 237 MPa Show Material materials with Streckgrenze of 237 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 247 MPa Show Material materials with Streckgrenze of 247 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
50 °C | 256 MPa Show Material materials with Streckgrenze of 256 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 168 MPa Show Material materials with Streckgrenze of 168 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 182 MPa Show Material materials with Streckgrenze of 182 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 196 MPa Show Material materials with Streckgrenze of 196 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 223 MPa Show Material materials with Streckgrenze of 223 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 232 MPa Show Material materials with Streckgrenze of 232 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
100 °C | 241 MPa Show Material materials with Streckgrenze of 241 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 156 MPa Show Material materials with Streckgrenze of 156 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 169 MPa Show Material materials with Streckgrenze of 169 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 181 MPa Show Material materials with Streckgrenze of 181 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 206 MPa Show Material materials with Streckgrenze of 206 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 215 MPa Show Material materials with Streckgrenze of 215 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
150 °C | 223 MPa Show Material materials with Streckgrenze of 223 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 143 MPa Show Material materials with Streckgrenze of 143 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 155 MPa Show Material materials with Streckgrenze of 155 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 167 MPa Show Material materials with Streckgrenze of 167 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 190 MPa Show Material materials with Streckgrenze of 190 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 197 MPa Show Material materials with Streckgrenze of 197 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
200 °C | 205 MPa Show Material materials with Streckgrenze of 205 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 131 MPa Show Material materials with Streckgrenze of 131 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 142 MPa Show Material materials with Streckgrenze of 142 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 153 MPa Show Material materials with Streckgrenze of 153 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 174 MPa Show Material materials with Streckgrenze of 174 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 181 MPa Show Material materials with Streckgrenze of 181 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
250 °C | 188 MPa Show Material materials with Streckgrenze of 188 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 121 MPa Show Material materials with Streckgrenze of 121 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 130 MPa Show Material materials with Streckgrenze of 130 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 140 MPa Show Material materials with Streckgrenze of 140 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 160 MPa Show Material materials with Streckgrenze of 160 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 166 MPa Show Material materials with Streckgrenze of 166 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
300 °C | 173 MPa Show Material materials with Streckgrenze of 173 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 112 MPa Show Material materials with Streckgrenze of 112 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 121 MPa Show Material materials with Streckgrenze of 121 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 130 MPa Show Material materials with Streckgrenze of 130 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 148 MPa Show Material materials with Streckgrenze of 148 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 154 MPa Show Material materials with Streckgrenze of 154 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
350 °C | 160 MPa Show Material materials with Streckgrenze of 160 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 105 MPa Show Material materials with Streckgrenze of 105 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 114 MPa Show Material materials with Streckgrenze of 114 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 122 MPa Show Material materials with Streckgrenze of 122 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 139 MPa Show Material materials with Streckgrenze of 139 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 145 MPa Show Material materials with Streckgrenze of 145 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
400 °C | 150 MPa Show Material materials with Streckgrenze of 150 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | RP02 | |
Zugfestigkeit | 20 °C | 390 - 530 MPa Show Material materials with Zugfestigkeit of 390 - 530 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse |
20 °C | 390 - 530 MPa Show Material materials with Zugfestigkeit of 390 - 530 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 400 - 530 MPa Show Material materials with Zugfestigkeit of 400 - 530 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 400 - 530 MPa Show Material materials with Zugfestigkeit of 400 - 530 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 410 - 530 MPa Show Material materials with Zugfestigkeit of 410 - 530 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat | Transverse | |
20 °C | 410 - 530 MPa Show Material materials with Zugfestigkeit of 410 - 530 MPa | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.08e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 1.19e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 1.25e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 1.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 1.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 1.45e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 1.49e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Max. Betriebstemperatur | 20 - 400 °C Show Material materials with Max. Betriebstemperatur of 20 - 400 °C | normalized or normalized formed (+N) | EN 10028-2 | Flat | Long | |
400 °C Show Material materials with Max. Betriebstemperatur of 400 °C | normalized or normalized formed (+N) | EN 10028-2 | Flat | Long | ||
500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | Typical for Carbon Steel | |||||
Schmelzpunkt | 1480 - 1526 °C Show Material materials with Schmelzpunkt of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Spezifische Wärmekapazität | -100 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 450 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 450 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 450 - 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 450 - 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Temperaturleitfähigkeit | 20 °C | 14.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 14.1 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
100 °C | 13.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 13.1 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 11.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 11.7 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 10.4 mm²/s Show Material materials with Temperaturleitfähigkeit of 10.4 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 9 mm²/s Show Material materials with Temperaturleitfähigkeit of 9 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 7.6 mm²/s Show Material materials with Temperaturleitfähigkeit of 7.6 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 6.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 6.1 mm²/s | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
Wärmeleitfähigkeit | 20 °C | 46.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 46.8 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
20 °C | 46.8 - 51 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 46.8 - 51 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
20 °C | 51 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 51 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 43 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 43 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 43 - 50.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 43 - 50.8 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
100 °C | 50.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 50.8 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 40 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 40 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 40 - 48.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 40 - 48.7 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 48.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 48.7 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 36 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 36 - 45.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36 - 45.8 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 45.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 45.8 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 32 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 32 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 32 - 42.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 32 - 42.5 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 42.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42.5 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 29 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 29 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 29 - 39.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 29 - 39.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 39.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 36 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36 W/(m·K) | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 6 S/m Show Material materials with Elektrische Leitfähigkeit of 6 S/m | Predicted Value | ||||
spezifischer Widerstand | 20 °C | 2.04e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.04e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
100 °C | 2.52e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.52e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
200 °C | 3.24e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.24e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
300 °C | 4.1e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.1e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
400 °C | 5.12e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.12e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
500 °C | 6.31e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.31e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat | ||
600 °C | 7.7e-07 Ω·m Show Material materials with spezifischer Widerstand of 7.7e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Magnetisch
Property | Value | Comment |
---|---|---|
Curie-Temperatur | 770 °C Show Material materials with Curie-Temperatur of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.02 % Show Material materials with Aluminium of 0.02 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Chrom | 0.3 % Show Material materials with Chrom of 0.3 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Kohlenstoff | 0.2 % Show Material materials with Kohlenstoff of 0.2 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Kupfer | 0.3 % Show Material materials with Kupfer of 0.3 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Mangan | 0.8 - 1.4 % Show Material materials with Mangan of 0.8 - 1.4 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Molybdän | 0.08 % Show Material materials with Molybdän of 0.08 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Nickel | 0.3 % Show Material materials with Nickel of 0.3 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Niobium | 0.02 % Show Material materials with Niobium of 0.02 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Phosphor | 0.025 % Show Material materials with Phosphor of 0.025 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Schwefel | 0.01 % Show Material materials with Schwefel of 0.01 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
0.015 % Show Material materials with Schwefel of 0.015 % | normalized or normalized formed (+N) | EN 10028-2 | Flat | |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Stickstoff | 0.012 % Show Material materials with Stickstoff of 0.012 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Titan | 0.03 % Show Material materials with Titan of 0.03 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Vanadium | 0.02 % Show Material materials with Vanadium of 0.02 % | normalized or normalized formed (+N) | EN 10028-2 | Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |