Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.83 - 7.84 g/cm³ Show Material materials with Dichte of 7.83 - 7.84 g/cm³ | normalized or normalized formed (+N) | EN 10028-3 | Flat |
20 °C | 7.83 g/cm³ Show Material materials with Dichte of 7.83 g/cm³ | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 7.84 g/cm³ Show Material materials with Dichte of 7.84 g/cm³ | normalized or normalized formed (+N) | EN 10028-3 | Flat |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 16.9 % Show Material materials with Dehnung of 16.9 % | Predicted Value, A80 Transverse | ||||
17.2 % Show Material materials with Dehnung of 17.2 % | Predicted Value, A80 | |||||
17.8 % Show Material materials with Dehnung of 17.8 % | Predicted Value, A200 | |||||
20.3 % Show Material materials with Dehnung of 20.3 % | Predicted Value, Transverse | |||||
20.6 % Show Material materials with Dehnung of 20.6 % | Predicted Value, A50 | |||||
21.2 % Show Material materials with Dehnung of 21.2 % | Predicted Value, A5 | |||||
20 °C | 20 % Show Material materials with Dehnung of 20 % | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | ||
20 °C | 21 % Show Material materials with Dehnung of 21 % | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 22 % Show Material materials with Dehnung of 22 % | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Elastizitätsmodul | -100 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 164 GPa Show Material materials with Elastizitätsmodul of 164 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Flächenreduzierung | 39.1 % Show Material materials with Flächenreduzierung of 39.1 % | Predicted Value | ||||
43.9 % Show Material materials with Flächenreduzierung of 43.9 % | Predicted Value, Transverse | |||||
Härte, Brinell | 240 [-] Show Material materials with Härte, Brinell of 240 [-] | Predicted Value, Transverse | ||||
Poissonzahl | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Low Carbon Steel | ||||
Scherfestigkeit | 516.8 MPa Show Material materials with Scherfestigkeit of 516.8 MPa | Predicted Value | ||||
Schubmodule | 82 GPa Show Material materials with Schubmodule of 82 GPa | Typical for Low Carbon Steel | ||||
Streckgrenze | 260.2 MPa Show Material materials with Streckgrenze of 260.2 MPa | Predicted Value, RP1 | ||||
315.1 MPa Show Material materials with Streckgrenze of 315.1 MPa | Predicted Value, RP1 Transverse | |||||
365.8 MPa Show Material materials with Streckgrenze of 365.8 MPa | Predicted Value, Transverse | |||||
458.1 MPa Show Material materials with Streckgrenze of 458.1 MPa | Predicted Value, RP02 Transverse | |||||
460.4 MPa Show Material materials with Streckgrenze of 460.4 MPa | Predicted Value, RP05 | |||||
464 MPa Show Material materials with Streckgrenze of 464 MPa | Predicted Value, RP002 | |||||
20 °C | 285 MPa Show Material materials with Streckgrenze of 285 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | ||
20 °C | 295 MPa Show Material materials with Streckgrenze of 295 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 305 MPa Show Material materials with Streckgrenze of 305 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 315 MPa Show Material materials with Streckgrenze of 315 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 335 MPa Show Material materials with Streckgrenze of 335 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 345 MPa Show Material materials with Streckgrenze of 345 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 355 MPa Show Material materials with Streckgrenze of 355 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
50 °C | 275 MPa Show Material materials with Streckgrenze of 275 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
50 °C | 285 MPa Show Material materials with Streckgrenze of 285 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 295 MPa Show Material materials with Streckgrenze of 295 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 305 MPa Show Material materials with Streckgrenze of 305 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 324 MPa Show Material materials with Streckgrenze of 324 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 334 MPa Show Material materials with Streckgrenze of 334 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 343 MPa Show Material materials with Streckgrenze of 343 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 245 MPa Show Material materials with Streckgrenze of 245 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
100 °C | 268 MPa Show Material materials with Streckgrenze of 268 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 277 MPa Show Material materials with Streckgrenze of 277 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 287 MPa Show Material materials with Streckgrenze of 287 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 305 MPa Show Material materials with Streckgrenze of 305 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 314 MPa Show Material materials with Streckgrenze of 314 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 323 MPa Show Material materials with Streckgrenze of 323 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 225 MPa Show Material materials with Streckgrenze of 225 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
150 °C | 249 MPa Show Material materials with Streckgrenze of 249 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 257 MPa Show Material materials with Streckgrenze of 257 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 265 MPa Show Material materials with Streckgrenze of 265 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 282 MPa Show Material materials with Streckgrenze of 282 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 291 MPa Show Material materials with Streckgrenze of 291 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 299 MPa Show Material materials with Streckgrenze of 299 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 206 MPa Show Material materials with Streckgrenze of 206 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
200 °C | 228 MPa Show Material materials with Streckgrenze of 228 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 236 MPa Show Material materials with Streckgrenze of 236 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 244 MPa Show Material materials with Streckgrenze of 244 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 259 MPa Show Material materials with Streckgrenze of 259 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 267 MPa Show Material materials with Streckgrenze of 267 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 275 MPa Show Material materials with Streckgrenze of 275 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
250 °C | 186 MPa Show Material materials with Streckgrenze of 186 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
250 °C | 209 MPa Show Material materials with Streckgrenze of 209 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 216 MPa Show Material materials with Streckgrenze of 216 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 224 MPa Show Material materials with Streckgrenze of 224 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 238 MPa Show Material materials with Streckgrenze of 238 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 245 MPa Show Material materials with Streckgrenze of 245 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
250 °C | 252 MPa Show Material materials with Streckgrenze of 252 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 167 MPa Show Material materials with Streckgrenze of 167 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
300 °C | 192 MPa Show Material materials with Streckgrenze of 192 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 199 MPa Show Material materials with Streckgrenze of 199 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 206 MPa Show Material materials with Streckgrenze of 206 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
300 °C | 219 MPa Show Material materials with Streckgrenze of 219 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 225 MPa Show Material materials with Streckgrenze of 225 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
300 °C | 232 MPa Show Material materials with Streckgrenze of 232 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 147 MPa Show Material materials with Streckgrenze of 147 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
350 °C | 178 MPa Show Material materials with Streckgrenze of 178 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 184 MPa Show Material materials with Streckgrenze of 184 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 190 MPa Show Material materials with Streckgrenze of 190 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 202 MPa Show Material materials with Streckgrenze of 202 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 208 MPa Show Material materials with Streckgrenze of 208 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 214 MPa Show Material materials with Streckgrenze of 214 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 117 MPa Show Material materials with Streckgrenze of 117 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
400 °C | 167 MPa Show Material materials with Streckgrenze of 167 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
400 °C | 173 MPa Show Material materials with Streckgrenze of 173 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 179 MPa Show Material materials with Streckgrenze of 179 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 190 MPa Show Material materials with Streckgrenze of 190 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 196 MPa Show Material materials with Streckgrenze of 196 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 202 MPa Show Material materials with Streckgrenze of 202 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
Zugfestigkeit | 20 °C | 440 - 590 MPa Show Material materials with Zugfestigkeit of 440 - 590 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | |
20 °C | 450 - 630 MPa Show Material materials with Zugfestigkeit of 450 - 630 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 450 - 610 MPa Show Material materials with Zugfestigkeit of 450 - 610 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 450 - 600 MPa Show Material materials with Zugfestigkeit of 450 - 600 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 450 - 590 MPa Show Material materials with Zugfestigkeit of 450 - 590 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 460 - 630 MPa Show Material materials with Zugfestigkeit of 460 - 630 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 460 - 610 MPa Show Material materials with Zugfestigkeit of 460 - 610 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 460 - 600 MPa Show Material materials with Zugfestigkeit of 460 - 600 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 460 - 590 MPa Show Material materials with Zugfestigkeit of 460 - 590 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 470 - 630 MPa Show Material materials with Zugfestigkeit of 470 - 630 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 470 - 610 MPa Show Material materials with Zugfestigkeit of 470 - 610 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 470 - 600 MPa Show Material materials with Zugfestigkeit of 470 - 600 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 470 - 590 MPa Show Material materials with Zugfestigkeit of 470 - 590 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 490 - 630 MPa Show Material materials with Zugfestigkeit of 490 - 630 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 490 - 610 MPa Show Material materials with Zugfestigkeit of 490 - 610 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 490 - 600 MPa Show Material materials with Zugfestigkeit of 490 - 600 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 490 - 590 MPa Show Material materials with Zugfestigkeit of 490 - 590 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.08e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 1.19e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 1.25e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 1.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 1.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 1.45e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 1.49e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Max. Betriebstemperatur | -20 - 400 °C Show Material materials with Max. Betriebstemperatur of -20 - 400 °C | normalized or normalized formed (+N) | EN 10028-3 | Flat | Long | |
400 °C Show Material materials with Max. Betriebstemperatur of 400 °C | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | Long | ||
500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | Typical for Carbon Steel | |||||
Schmelzpunkt | 1480 - 1526 °C Show Material materials with Schmelzpunkt of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Spezifische Wärmekapazität | -100 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 430 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 430 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 430 - 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 430 - 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Temperaturleitfähigkeit | -100 °C | 12.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 12.9 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 11.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 11.7 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 11.2 mm²/s Show Material materials with Temperaturleitfähigkeit of 11.2 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 10.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 10.3 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 9.4 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.4 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 8.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.3 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 7.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 7.1 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 5.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.7 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Wärmeleitfähigkeit | -100 °C | 37.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 37.6 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 42 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 42 - 42.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42 - 42.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 42.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 43.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 43.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 42.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42.9 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 41.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 41.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 39.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39.1 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 36.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36.6 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 34.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 34.1 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 5 S/m Show Material materials with Elektrische Leitfähigkeit of 5 S/m | Predicted Value | ||||
spezifischer Widerstand | -100 °C | 1.82e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.82e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 2.47e-07 - 2.5e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.47e-07 - 2.5e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 2.47e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.47e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 2.5e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.5e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 2.96e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.96e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 3.68e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.68e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 4.55e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.55e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 5.56e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.56e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 6.75e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.75e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 8.13e-07 Ω·m Show Material materials with spezifischer Widerstand of 8.13e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat |
Magnetisch
Property | Value | Comment |
---|---|---|
Curie-Temperatur | 770 °C Show Material materials with Curie-Temperatur of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.02 % Show Material materials with Aluminium of 0.02 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Chrom | 0.3 % Show Material materials with Chrom of 0.3 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Kohlenstoff | 0.18 % Show Material materials with Kohlenstoff of 0.18 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Kupfer | 0.3 % Show Material materials with Kupfer of 0.3 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Mangan | 1.1 - 1.7 % Show Material materials with Mangan of 1.1 - 1.7 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Molybdän | 0.08 % Show Material materials with Molybdän of 0.08 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Nickel | 0.5 % Show Material materials with Nickel of 0.5 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Niobium | 0.05 % Show Material materials with Niobium of 0.05 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Phosphor | 0.025 % Show Material materials with Phosphor of 0.025 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Schwefel | 0.015 % Show Material materials with Schwefel of 0.015 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Silizium | 0.5 % Show Material materials with Silizium of 0.5 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Stickstoff | 0.012 % Show Material materials with Stickstoff of 0.012 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Titan | 0.03 % Show Material materials with Titan of 0.03 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Vanadium | 0.1 % Show Material materials with Vanadium of 0.1 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |