Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.84 g/cm³ Show Material materials with Dichte of 7.84 g/cm³ | normalized and stress-relieved | EN 10028-3 | Sheet |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastizitätsmodul | -100 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | |
20 °C | 200 - 212 GPa Show Material materials with Elastizitätsmodul of 200 - 212 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
20 °C | 200 GPa Show Material materials with Elastizitätsmodul of 200 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
20 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
100 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
200 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
300 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
400 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
500 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
600 °C | 164 GPa Show Material materials with Elastizitätsmodul of 164 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | ||
Poissonzahl | 20 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | normalized and stress-relieved | EN 10028-3 | Sheet | |
Schubmodule | 82 GPa Show Material materials with Schubmodule of 82 GPa | Typical for Low Carbon Steel |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.05e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | |
20 °C | 1.15e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.15e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | ||
100 °C | 1.21e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | ||
200 °C | 1.27e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | ||
300 °C | 1.32e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | ||
400 °C | 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | ||
500 °C | 1.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | ||
600 °C | 1.44e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.44e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | ||
Max. Betriebstemperatur | 500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | Typical for Carbon Steel | ||||
Schmelzpunkt | 1480 - 1526 °C Show Material materials with Schmelzpunkt of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Spezifische Wärmekapazität | -100 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | |
20 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
200 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
300 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
400 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
500 °C | 558 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
600 °C | 587 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
Temperaturleitfähigkeit | -100 °C | 11.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 11.9 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | |
20 °C | 11 mm²/s Show Material materials with Temperaturleitfähigkeit of 11 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | ||
100 °C | 10.5 mm²/s Show Material materials with Temperaturleitfähigkeit of 10.5 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | ||
200 °C | 9.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.9 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | ||
300 °C | 9.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.1 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | ||
400 °C | 8.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.1 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | ||
500 °C | 6.9 mm²/s Show Material materials with Temperaturleitfähigkeit of 6.9 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | ||
600 °C | 5.7 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.7 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | ||
Wärmeleitfähigkeit | -100 °C | 34.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 34.7 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | |
20 °C | 39.7 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39.7 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
100 °C | 40.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 40.9 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
200 °C | 41 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 41 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
300 °C | 39.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 39.9 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
400 °C | 38.2 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38.2 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
500 °C | 36.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36.1 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | ||
600 °C | 33.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 33.8 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
spezifischer Widerstand | -100 °C | 1.97e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.97e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet |
20 °C | 2.62e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.62e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet | |
100 °C | 3.13e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.13e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet | |
200 °C | 3.85e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.85e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet | |
300 °C | 4.7e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.7e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet | |
400 °C | 5.69e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.69e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet | |
500 °C | 6.85e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.85e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet | |
600 °C | 8.2e-07 Ω·m Show Material materials with spezifischer Widerstand of 8.2e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet |
Magnetisch
Property | Value | Comment |
---|---|---|
Curie-Temperatur | 770 °C Show Material materials with Curie-Temperatur of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.005 % Show Material materials with Aluminium of 0.005 % | normalized and stress-relieved | EN 10028-3 | Sheet |
Chrom | 0.3 Show Material materials with Chrom of 0.3 | normalized and stress-relieved | EN 10028-3 | Sheet |
Kohlenstoff | 0.2 Show Material materials with Kohlenstoff of 0.2 | normalized and stress-relieved | EN 10028-3 | Sheet |
Kupfer | 0.2 Show Material materials with Kupfer of 0.2 | normalized and stress-relieved | EN 10028-3 | Sheet |
Mangan | 1 - 1.7 % Show Material materials with Mangan of 1 - 1.7 % | normalized and stress-relieved | EN 10028-3 | Sheet |
Molybdän | 0.1 Show Material materials with Molybdän of 0.1 | normalized and stress-relieved | EN 10028-3 | Sheet |
Nickel | 0.4 Show Material materials with Nickel of 0.4 | normalized and stress-relieved | EN 10028-3 | Sheet |
Phosphor | 0.03 Show Material materials with Phosphor of 0.03 | normalized and stress-relieved | EN 10028-3 | Sheet |
Schwefel | 0.02 Show Material materials with Schwefel of 0.02 | normalized and stress-relieved | EN 10028-3 | Sheet |
Silizium | 0.1 - 0.6 % Show Material materials with Silizium of 0.1 - 0.6 % | normalized and stress-relieved | EN 10028-3 | Sheet |
Stickstoff | 0.025 Show Material materials with Stickstoff of 0.025 | normalized and stress-relieved | EN 10028-3 | Sheet |
Vanadium | 0.1 - 0.2 % Show Material materials with Vanadium of 0.1 - 0.2 % | normalized and stress-relieved | EN 10028-3 | Sheet |