Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 7.8 g/cm³ Show Material materials with Dichte of 7.8 g/cm³ | Typical for Steel |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 15.7 % Show Material materials with Dehnung of 15.7 % | Predicted Value, A80 | ||||
15.7 % Show Material materials with Dehnung of 15.7 % | Predicted Value, A200 | |||||
17.5 % Show Material materials with Dehnung of 17.5 % | Predicted Value, Transverse | |||||
18.2 % Show Material materials with Dehnung of 18.2 % | Predicted Value, A80 Transverse | |||||
20.9 % Show Material materials with Dehnung of 20.9 % | Predicted Value, A5 | |||||
23.3 % Show Material materials with Dehnung of 23.3 % | Predicted Value, A50 | |||||
20 °C | 16 % Show Material materials with Dehnung of 16 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 17 % Show Material materials with Dehnung of 17 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Elastizitätsmodul | 190 - 210 GPa Show Material materials with Elastizitätsmodul of 190 - 210 GPa | Typical for Steel | ||||
Flächenreduzierung | 43.8 % Show Material materials with Flächenreduzierung of 43.8 % | Predicted Value, Transverse | ||||
51.5 % Show Material materials with Flächenreduzierung of 51.5 % | Predicted Value | |||||
Härte, Brinell | 251 [-] Show Material materials with Härte, Brinell of 251 [-] | Predicted Value, Transverse | ||||
Poissonzahl | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Steel | ||||
Scherfestigkeit | 527.8 MPa Show Material materials with Scherfestigkeit of 527.8 MPa | Predicted Value | ||||
Schubmodule | 80.3 GPa Show Material materials with Schubmodule of 80.3 GPa | Predicted Value | ||||
Streckgrenze | 260.4 MPa Show Material materials with Streckgrenze of 260.4 MPa | Predicted Value, RP1 | ||||
319.7 MPa Show Material materials with Streckgrenze of 319.7 MPa | Predicted Value, RP1 Transverse | |||||
408.4 MPa Show Material materials with Streckgrenze of 408.4 MPa | Predicted Value, Transverse | |||||
430.6 MPa Show Material materials with Streckgrenze of 430.6 MPa | Predicted Value, RP02 | |||||
470 MPa Show Material materials with Streckgrenze of 470 MPa | Predicted Value, RP02 Transverse | |||||
495.2 MPa Show Material materials with Streckgrenze of 495.2 MPa | Predicted Value, RP002 | |||||
526.7 MPa Show Material materials with Streckgrenze of 526.7 MPa | Predicted Value, RP05 | |||||
20 °C | 370 MPa Show Material materials with Streckgrenze of 370 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 380 MPa Show Material materials with Streckgrenze of 380 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 400 MPa Show Material materials with Streckgrenze of 400 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 410 MPa Show Material materials with Streckgrenze of 410 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 430 MPa Show Material materials with Streckgrenze of 430 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 440 MPa Show Material materials with Streckgrenze of 440 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 460 MPa Show Material materials with Streckgrenze of 460 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Zugfestigkeit | 20 °C | 510 - 720 MPa Show Material materials with Zugfestigkeit of 510 - 720 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 510 - 700 MPa Show Material materials with Zugfestigkeit of 510 - 700 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 510 - 690 MPa Show Material materials with Zugfestigkeit of 510 - 690 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 520 - 690 MPa Show Material materials with Zugfestigkeit of 520 - 690 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Flat | ||
20 °C | 530 - 720 MPa Show Material materials with Zugfestigkeit of 530 - 720 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 530 - 700 MPa Show Material materials with Zugfestigkeit of 530 - 700 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 530 - 690 MPa Show Material materials with Zugfestigkeit of 530 - 690 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 550 - 720 MPa Show Material materials with Zugfestigkeit of 550 - 720 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 550 - 700 MPa Show Material materials with Zugfestigkeit of 550 - 700 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 550 - 690 MPa Show Material materials with Zugfestigkeit of 550 - 690 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 11.82 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 11.82 1/K | Predicted Value |
Spezifische Wärmekapazität | 454.3 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 454.3 J/(kg·K) | Predicted Value |
Wärmeleitfähigkeit | 38.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38.3 W/(m·K) | Predicted Value |
Elektrisch
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.02 % Show Material materials with Aluminium of 0.02 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Chrom | 0.3 % Show Material materials with Chrom of 0.3 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Kohlenstoff | 0.2 % Show Material materials with Kohlenstoff of 0.2 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Kupfer | 0.55 % Show Material materials with Kupfer of 0.55 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
0.7 % Show Material materials with Kupfer of 0.7 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat | |
Mangan | 1 - 1.7 % Show Material materials with Mangan of 1 - 1.7 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Molybdän | 0.1 % Show Material materials with Molybdän of 0.1 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Nickel | 0.8 % Show Material materials with Nickel of 0.8 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Niobium | 0.05 % Show Material materials with Niobium of 0.05 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat |
0.2 % Show Material materials with Niobium of 0.2 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | |
Phosphor | 0.03 % Show Material materials with Phosphor of 0.03 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
0.035 % Show Material materials with Phosphor of 0.035 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat | |
Schwefel | 0.025 % Show Material materials with Schwefel of 0.025 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
0.03 % Show Material materials with Schwefel of 0.03 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat | |
Silizium | 0.6 % Show Material materials with Silizium of 0.6 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Stickstoff | 0.025 % Show Material materials with Stickstoff of 0.025 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Titan | 0.03 % Show Material materials with Titan of 0.03 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat |
0.05 % Show Material materials with Titan of 0.05 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | |
Vanadium | 0.05 % Show Material materials with Vanadium of 0.05 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
0.2 % Show Material materials with Vanadium of 0.2 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |