Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20 °C | 7.84 g/cm³ Show Material materials with Dichte of 7.84 g/cm³ | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 16.4 % Show Material materials with Dehnung of 16.4 % | Predicted Value, A80 Transverse | ||||
16.6 % Show Material materials with Dehnung of 16.6 % | Predicted Value, A80 | |||||
17 % Show Material materials with Dehnung of 17 % | Predicted Value, A200 | |||||
18.8 % Show Material materials with Dehnung of 18.8 % | Predicted Value, Transverse | |||||
20.9 % Show Material materials with Dehnung of 20.9 % | Predicted Value, A50 | |||||
21.1 % Show Material materials with Dehnung of 21.1 % | Predicted Value, A5 | |||||
20 °C | 17 % Show Material materials with Dehnung of 17 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Flat | ||
20 °C | 18 % Show Material materials with Dehnung of 18 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 19 % Show Material materials with Dehnung of 19 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
Elastizitätsmodul | -100 °C | 217 GPa Show Material materials with Elastizitätsmodul of 217 GPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | |
20 °C | 212 GPa Show Material materials with Elastizitätsmodul of 212 GPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
100 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
200 °C | 199 GPa Show Material materials with Elastizitätsmodul of 199 GPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
300 °C | 192 GPa Show Material materials with Elastizitätsmodul of 192 GPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
400 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
500 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
600 °C | 164 GPa Show Material materials with Elastizitätsmodul of 164 GPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Flächenreduzierung | 44.1 % Show Material materials with Flächenreduzierung of 44.1 % | Predicted Value, Transverse | ||||
50.8 % Show Material materials with Flächenreduzierung of 50.8 % | Predicted Value | |||||
Härte, Brinell | 247 [-] Show Material materials with Härte, Brinell of 247 [-] | Predicted Value, Transverse | ||||
Poissonzahl | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Low Carbon Steel | ||||
Scherfestigkeit | 510.8 MPa Show Material materials with Scherfestigkeit of 510.8 MPa | Predicted Value | ||||
Schubmodule | 82 GPa Show Material materials with Schubmodule of 82 GPa | Typical for Low Carbon Steel | ||||
Streckgrenze | 257.3 MPa Show Material materials with Streckgrenze of 257.3 MPa | Predicted Value, RP1 | ||||
301.6 MPa Show Material materials with Streckgrenze of 301.6 MPa | Predicted Value, RP1 Transverse | |||||
397.1 MPa Show Material materials with Streckgrenze of 397.1 MPa | Predicted Value, Transverse | |||||
413.2 MPa Show Material materials with Streckgrenze of 413.2 MPa | Predicted Value, RP02 | |||||
456.3 MPa Show Material materials with Streckgrenze of 456.3 MPa | Predicted Value, RP02 Transverse | |||||
480.4 MPa Show Material materials with Streckgrenze of 480.4 MPa | Predicted Value, RP002 | |||||
499.9 MPa Show Material materials with Streckgrenze of 499.9 MPa | Predicted Value, RP05 | |||||
20 °C | 320 MPa Show Material materials with Streckgrenze of 320 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 330 MPa Show Material materials with Streckgrenze of 330 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 335 MPa Show Material materials with Streckgrenze of 335 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Flat | ||
20 °C | 340 MPa Show Material materials with Streckgrenze of 340 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 360 MPa Show Material materials with Streckgrenze of 360 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 370 MPa Show Material materials with Streckgrenze of 370 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 390 MPa Show Material materials with Streckgrenze of 390 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 400 MPa Show Material materials with Streckgrenze of 400 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 420 MPa Show Material materials with Streckgrenze of 420 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
Zugfestigkeit | 20 °C | 480 - 640 MPa Show Material materials with Zugfestigkeit of 480 - 640 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Flat | |
20 °C | 500 - 680 MPa Show Material materials with Zugfestigkeit of 500 - 680 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 500 - 650 MPa Show Material materials with Zugfestigkeit of 500 - 650 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 520 - 680 MPa Show Material materials with Zugfestigkeit of 520 - 680 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire | ||
20 °C | 520 - 650 MPa Show Material materials with Zugfestigkeit of 520 - 650 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat, Rod, Wire |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -100 °C | 1.05e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.05e-05 1/K | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | |
20 °C | 1.15e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.15e-05 1/K | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
100 °C | 1.21e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.21e-05 1/K | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
200 °C | 1.27e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.27e-05 1/K | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
300 °C | 1.32e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 1/K | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
400 °C | 1.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
500 °C | 1.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.4e-05 1/K | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
600 °C | 1.44e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.44e-05 1/K | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Max. Betriebstemperatur | 218.6 °C Show Material materials with Max. Betriebstemperatur of 218.6 °C | Predicted Value, Long | ||||
500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | Typical for Carbon Steel | |||||
Schmelzpunkt | 1480 - 1526 °C Show Material materials with Schmelzpunkt of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Spezifische Wärmekapazität | -100 °C | 423 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | |
20 °C | 461 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
100 °C | 479 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
200 °C | 499 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
300 °C | 517 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
400 °C | 536 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
500 °C | 558 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
600 °C | 587 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Temperaturleitfähigkeit | -100 °C | 12.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 12.1 mm²/s | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | |
20 °C | 11.2 mm²/s Show Material materials with Temperaturleitfähigkeit of 11.2 mm²/s | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
100 °C | 10.8 mm²/s Show Material materials with Temperaturleitfähigkeit of 10.8 mm²/s | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
200 °C | 10.1 mm²/s Show Material materials with Temperaturleitfähigkeit of 10.1 mm²/s | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
300 °C | 9.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 9.3 mm²/s | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
400 °C | 8.3 mm²/s Show Material materials with Temperaturleitfähigkeit of 8.3 mm²/s | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
500 °C | 7 mm²/s Show Material materials with Temperaturleitfähigkeit of 7 mm²/s | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
600 °C | 5.8 mm²/s Show Material materials with Temperaturleitfähigkeit of 5.8 mm²/s | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Wärmeleitfähigkeit | -100 °C | 35.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 35.4 W/(m·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | |
20 °C | 40.4 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 40.4 W/(m·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
100 °C | 42 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42 W/(m·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
200 °C | 42 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 42 W/(m·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
300 °C | 40.8 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 40.8 W/(m·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
400 °C | 38.9 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38.9 W/(m·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
500 °C | 36.6 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36.6 W/(m·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
600 °C | 34.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 34.3 W/(m·K) | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 5 S/m Show Material materials with Elektrische Leitfähigkeit of 5 S/m | Predicted Value | ||||
spezifischer Widerstand | -100 °C | 1.93e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.93e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | |
20 °C | 2.58e-07 Ω·m Show Material materials with spezifischer Widerstand of 2.58e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
100 °C | 3.05e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.05e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
200 °C | 3.76e-07 Ω·m Show Material materials with spezifischer Widerstand of 3.76e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
300 °C | 4.6e-07 Ω·m Show Material materials with spezifischer Widerstand of 4.6e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
400 °C | 5.59e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.59e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
500 °C | 6.75e-07 Ω·m Show Material materials with spezifischer Widerstand of 6.75e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
600 °C | 8.08e-07 Ω·m Show Material materials with spezifischer Widerstand of 8.08e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Magnetisch
Property | Value | Comment |
---|---|---|
Curie-Temperatur | 770 °C Show Material materials with Curie-Temperatur of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 0.02 % Show Material materials with Aluminium of 0.02 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Chrom | 0.3 % Show Material materials with Chrom of 0.3 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Kohlenstoff | 0.2 % Show Material materials with Kohlenstoff of 0.2 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Kupfer | 0.55 % Show Material materials with Kupfer of 0.55 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
0.7 % Show Material materials with Kupfer of 0.7 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat | |
Mangan | 1 - 1.7 % Show Material materials with Mangan of 1 - 1.7 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Molybdän | 0.1 % Show Material materials with Molybdän of 0.1 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Nickel | 0.8 % Show Material materials with Nickel of 0.8 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Niobium | 0.05 % Show Material materials with Niobium of 0.05 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat |
0.2 % Show Material materials with Niobium of 0.2 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | |
Phosphor | 0.03 % Show Material materials with Phosphor of 0.03 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
0.035 % Show Material materials with Phosphor of 0.035 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat | |
Schwefel | 0.025 % Show Material materials with Schwefel of 0.025 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
0.03 % Show Material materials with Schwefel of 0.03 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat | |
Silizium | 0.6 % Show Material materials with Silizium of 0.6 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Stickstoff | 0.025 % Show Material materials with Stickstoff of 0.025 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Titan | 0.03 % Show Material materials with Titan of 0.03 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat |
0.05 % Show Material materials with Titan of 0.05 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | |
Vanadium | 0.05 % Show Material materials with Vanadium of 0.05 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
0.2 % Show Material materials with Vanadium of 0.2 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |