Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 7.8 - 7.9 g/cm³ Show Material materials with Dichte of 7.8 - 7.9 g/cm³ | Typical for Low Carbon Steel |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 14.4 % Show Material materials with Dehnung of 14.4 % | Predicted Value, A200 | ||||
20.1 % Show Material materials with Dehnung of 20.1 % | Predicted Value, A5 | |||||
20.6 % Show Material materials with Dehnung of 20.6 % | Predicted Value, A50 | |||||
20.8 % Show Material materials with Dehnung of 20.8 % | Predicted Value, Transverse | |||||
21.0 % Show Material materials with Dehnung of 21.0 % | Predicted Value | |||||
20 °C | 26 % Show Material materials with Dehnung of 26 % | cold rolled, skin passed | EN 10209 | Sheet | A80 Transverse | |
20 °C | 28 % Show Material materials with Dehnung of 28 % | cold rolled, skin passed | EN 10209 | Sheet | A80 Transverse | |
20 °C | 30 % Show Material materials with Dehnung of 30 % | cold rolled, skin passed | EN 10209 | Sheet | A80 Transverse | |
20 °C | 30 % Show Material materials with Dehnung of 30 % | cold rolled, skin passed | EN 10209 | Strip, Bar | A80 | |
Elastizitätsmodul | 200 - 215 GPa Show Material materials with Elastizitätsmodul of 200 - 215 GPa | Typical for Low Carbon Steel | ||||
Flächenreduzierung | 40.0 % Show Material materials with Flächenreduzierung of 40.0 % | Predicted Value | ||||
43.6 % Show Material materials with Flächenreduzierung of 43.6 % | Predicted Value, Transverse | |||||
Härte, Brinell | 261 [-] Show Material materials with Härte, Brinell of 261 [-] | Predicted Value, Transverse | ||||
Poissonzahl | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Low Carbon Steel | ||||
Scherfestigkeit | 527 MPa Show Material materials with Scherfestigkeit of 527 MPa | Predicted Value | ||||
Schubmodule | 82 GPa Show Material materials with Schubmodule of 82 GPa | Typical for Low Carbon Steel | ||||
Streckgrenze | 277.9 MPa Show Material materials with Streckgrenze of 277.9 MPa | Predicted Value, RP05 | ||||
285.1 MPa Show Material materials with Streckgrenze of 285.1 MPa | Predicted Value, RP1 Transverse | |||||
293.6 MPa Show Material materials with Streckgrenze of 293.6 MPa | Predicted Value, RP1 | |||||
365.5 MPa Show Material materials with Streckgrenze of 365.5 MPa | Predicted Value, RP02 Transverse | |||||
538.6 MPa Show Material materials with Streckgrenze of 538.6 MPa | Predicted Value, RP02 | |||||
626.3 MPa Show Material materials with Streckgrenze of 626.3 MPa | Predicted Value, RP002 | |||||
20 °C | 140 - 310 MPa Show Material materials with Streckgrenze of 140 - 310 MPa | cold rolled, skin passed | EN 10209 | Sheet | Transverse | |
20 °C | 140 - 290 MPa Show Material materials with Streckgrenze of 140 - 290 MPa | cold rolled, skin passed | EN 10209 | Sheet | Transverse | |
20 °C | 140 - 270 MPa Show Material materials with Streckgrenze of 140 - 270 MPa | cold rolled, skin passed | EN 10209 | Sheet | Transverse | |
20 °C | 140 - 270 MPa Show Material materials with Streckgrenze of 140 - 270 MPa | cold rolled, skin passed | EN 10209 | Strip, Bar | ||
Zugfestigkeit | 20 °C | 270 - 390 MPa Show Material materials with Zugfestigkeit of 270 - 390 MPa | cold rolled, skin passed | EN 10209 | Sheet | Transverse |
20 °C | 270 - 390 MPa Show Material materials with Zugfestigkeit of 270 - 390 MPa | cold rolled, skin passed | EN 10209 | Strip, Bar |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 1.32e-05 - 1.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.32e-05 - 1.38e-05 1/K | Typical for Low Carbon Steel |
Max. Betriebstemperatur | 330.7 °C Show Material materials with Max. Betriebstemperatur of 330.7 °C | Predicted Value, Long |
500 °C Show Material materials with Max. Betriebstemperatur of 500 °C | Typical for Carbon Steel | |
Schmelzpunkt | 1480 - 1526 °C Show Material materials with Schmelzpunkt of 1480 - 1526 °C | Typical for Low Carbon Steel |
Spezifische Wärmekapazität | 465 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 465 J/(kg·K) | Typical for Low Carbon Steel |
Wärmeleitfähigkeit | 25 - 93 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 25 - 93 W/(m·K) | Typical for Low Carbon Steel |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 8 S/m Show Material materials with Elektrische Leitfähigkeit of 8 S/m | Predicted Value |
spezifischer Widerstand | 1.43e-07 - 1.74e-07 Ω·m Show Material materials with spezifischer Widerstand of 1.43e-07 - 1.74e-07 Ω·m | Typical for Carbon Steel |
Magnetisch
Property | Value | Comment |
---|---|---|
Curie-Temperatur | 770 °C Show Material materials with Curie-Temperatur of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Kohlenstoff | 0.08 % Show Material materials with Kohlenstoff of 0.08 % | cold rolled, skin passed | EN 10209 | Sheet |
Mangan | 0.6 % Show Material materials with Mangan of 0.6 % | cold rolled, skin passed | EN 10209 | Sheet |
Phosphor | 0.045 % Show Material materials with Phosphor of 0.045 % | cold rolled, skin passed | EN 10209 | Sheet |
Schwefel | 0.05 % Show Material materials with Schwefel of 0.05 % | cold rolled, skin passed | EN 10209 | Sheet |