Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8 g/cm³ Show Material materials with Dichte of 8 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung A80, transversal | 20.0 °C | 35 - 40 % Show Material materials with Dehnung A80, transversal of 35 - 40 % | |
Dehnung, transversal | 20.0 °C | 35 - 40 % Show Material materials with Dehnung, transversal of 35 - 40 % | |
Elastizitätsmodul | 20.0 °C | 200 GPa Show Material materials with Elastizitätsmodul of 200 GPa | |
100.0 °C | 194 GPa Show Material materials with Elastizitätsmodul of 194 GPa | ||
200.0 °C | 186 GPa Show Material materials with Elastizitätsmodul of 186 GPa | ||
300.0 °C | 179 GPa Show Material materials with Elastizitätsmodul of 179 GPa | ||
400.0 °C | 172 GPa Show Material materials with Elastizitätsmodul of 172 GPa | ||
500.0 °C | 165 GPa Show Material materials with Elastizitätsmodul of 165 GPa | ||
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Austenitic Stainless Steel |
Schubmodule | 23.0 °C | 77 GPa Show Material materials with Schubmodule of 77 GPa | Typical for Austenitic Stainless Steel |
Streckgrenze Rp 0,2 | 50.0 °C | 248 MPa Show Material materials with Streckgrenze Rp 0,2 of 248 MPa | |
100.0 °C | 211 MPa Show Material materials with Streckgrenze Rp 0,2 of 211 MPa | ||
150.0 °C | 185 MPa Show Material materials with Streckgrenze Rp 0,2 of 185 MPa | ||
200.0 °C | 167 MPa Show Material materials with Streckgrenze Rp 0,2 of 167 MPa | ||
250.0 °C | 155 MPa Show Material materials with Streckgrenze Rp 0,2 of 155 MPa | ||
300.0 °C | 145 MPa Show Material materials with Streckgrenze Rp 0,2 of 145 MPa | ||
350.0 °C | 140 MPa Show Material materials with Streckgrenze Rp 0,2 of 140 MPa | ||
400.0 °C | 135 MPa Show Material materials with Streckgrenze Rp 0,2 of 135 MPa | ||
450.0 °C | 131 MPa Show Material materials with Streckgrenze Rp 0,2 of 131 MPa | ||
500.0 °C | 129 MPa Show Material materials with Streckgrenze Rp 0,2 of 129 MPa | ||
550.0 °C | 127 MPa Show Material materials with Streckgrenze Rp 0,2 of 127 MPa | ||
Streckgrenze Rp 0,2, transversal | 20.0 °C | 270 - 290 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 270 - 290 MPa | |
Streckgrenze Rp 1,0 | 50.0 °C | 286 MPa Show Material materials with Streckgrenze Rp 1,0 of 286 MPa | |
100.0 °C | 246 MPa Show Material materials with Streckgrenze Rp 1,0 of 246 MPa | ||
150.0 °C | 218 MPa Show Material materials with Streckgrenze Rp 1,0 of 218 MPa | ||
200.0 °C | 198 MPa Show Material materials with Streckgrenze Rp 1,0 of 198 MPa | ||
250.0 °C | 183 MPa Show Material materials with Streckgrenze Rp 1,0 of 183 MPa | ||
300.0 °C | 175 MPa Show Material materials with Streckgrenze Rp 1,0 of 175 MPa | ||
350.0 °C | 169 MPa Show Material materials with Streckgrenze Rp 1,0 of 169 MPa | ||
400.0 °C | 164 MPa Show Material materials with Streckgrenze Rp 1,0 of 164 MPa | ||
450.0 °C | 160 MPa Show Material materials with Streckgrenze Rp 1,0 of 160 MPa | ||
500.0 °C | 158 MPa Show Material materials with Streckgrenze Rp 1,0 of 158 MPa | ||
550.0 °C | 157 MPa Show Material materials with Streckgrenze Rp 1,0 of 157 MPa | ||
Streckgrenze Rp 1,0, transversal | 20.0 °C | 310 - 320 MPa Show Material materials with Streckgrenze Rp 1,0, transversal of 310 - 320 MPa | |
Zugfestigkeit | 20.0 °C | 540 - 770 MPa Show Material materials with Zugfestigkeit of 540 - 770 MPa | |
50.0 °C | 525 MPa Show Material materials with Zugfestigkeit of 525 MPa | ||
100.0 °C | 500 MPa Show Material materials with Zugfestigkeit of 500 MPa | ||
150.0 °C | 470 MPa Show Material materials with Zugfestigkeit of 470 MPa | ||
200.0 °C | 440 MPa Show Material materials with Zugfestigkeit of 440 MPa | ||
250.0 °C | 430 MPa Show Material materials with Zugfestigkeit of 430 MPa | ||
300.0 °C | 420 MPa Show Material materials with Zugfestigkeit of 420 MPa | ||
350.0 °C | 415 MPa Show Material materials with Zugfestigkeit of 415 MPa | ||
400.0 °C | 415 MPa Show Material materials with Zugfestigkeit of 415 MPa | ||
450.0 °C | 415 MPa Show Material materials with Zugfestigkeit of 415 MPa | ||
500.0 °C | 410 MPa Show Material materials with Zugfestigkeit of 410 MPa | ||
550.0 °C | 390 MPa Show Material materials with Zugfestigkeit of 390 MPa | ||
Zugfestigkeit, transversal | 20.0 °C | 540 - 770 MPa Show Material materials with Zugfestigkeit, transversal of 540 - 770 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.6E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6E-5 1/K | |
200.0 °C | 1.65E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.65E-5 1/K | ||
300.0 °C | 1.7E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 1/K | ||
400.0 °C | 1.75E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.75E-5 1/K | ||
500.0 °C | 1.8E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.8E-5 1/K | ||
Schmelzpunkt | 1230 - 1480 °C Show Material materials with Schmelzpunkt of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Spezifische Wärmekapazität | 20.0 °C | 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 500 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 15 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 15 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 7.5E-7 Ω·m Show Material materials with spezifischer Widerstand of 7.5E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Chrom | 16.5 - 19.5 % Show Material materials with Chrom of 16.5 - 19.5 % |
Kohlenstoff | 0.03 % Show Material materials with Kohlenstoff of 0.03 % |
Mangan | 2 % Show Material materials with Mangan of 2 % |
Molybdän | 3 - 4 % Show Material materials with Molybdän of 3 - 4 % |
Nickel | 10.5 - 14 % Show Material materials with Nickel of 10.5 - 14 % |
Phosphor | 0.05 % Show Material materials with Phosphor of 0.05 % |
Schwefel | 0.015 % Show Material materials with Schwefel of 0.015 % |
Silizium | 1 % Show Material materials with Silizium of 1 % |
Stickstoff | 0.1 - 0.2 % Show Material materials with Stickstoff of 0.1 - 0.2 % |