Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8.1 g/cm³ Show Material materials with Dichte of 8.1 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung A80, transversal | 20.0 °C | 40 % Show Material materials with Dehnung A80, transversal of 40 % | |
Dehnung, transversal | 20.0 °C | 40 % Show Material materials with Dehnung, transversal of 40 % | |
Elastizitätsmodul | 20.0 °C | 195 GPa Show Material materials with Elastizitätsmodul of 195 GPa | |
100.0 °C | 190 GPa Show Material materials with Elastizitätsmodul of 190 GPa | ||
200.0 °C | 182 GPa Show Material materials with Elastizitätsmodul of 182 GPa | ||
300.0 °C | 174 GPa Show Material materials with Elastizitätsmodul of 174 GPa | ||
400.0 °C | 166 GPa Show Material materials with Elastizitätsmodul of 166 GPa | ||
500.0 °C | 158 GPa Show Material materials with Elastizitätsmodul of 158 GPa | ||
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Austenitic Stainless Steel |
Schubmodule | 23.0 °C | 77 GPa Show Material materials with Schubmodule of 77 GPa | Typical for Austenitic Stainless Steel |
Streckgrenze Rp 0,2 | 50.0 °C | 271 MPa Show Material materials with Streckgrenze Rp 0,2 of 271 MPa | |
100.0 °C | 240 MPa Show Material materials with Streckgrenze Rp 0,2 of 240 MPa | ||
150.0 °C | 220 MPa Show Material materials with Streckgrenze Rp 0,2 of 220 MPa | ||
200.0 °C | 200 MPa Show Material materials with Streckgrenze Rp 0,2 of 200 MPa | ||
250.0 °C | 190 MPa Show Material materials with Streckgrenze Rp 0,2 of 190 MPa | ||
300.0 °C | 180 MPa Show Material materials with Streckgrenze Rp 0,2 of 180 MPa | ||
350.0 °C | 175 MPa Show Material materials with Streckgrenze Rp 0,2 of 175 MPa | ||
400.0 °C | 170 MPa Show Material materials with Streckgrenze Rp 0,2 of 170 MPa | ||
Streckgrenze Rp 0,2, transversal | 20.0 °C | 290 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 290 MPa | |
Streckgrenze Rp 1,0 | 50.0 °C | 307 MPa Show Material materials with Streckgrenze Rp 1,0 of 307 MPa | |
100.0 °C | 270 MPa Show Material materials with Streckgrenze Rp 1,0 of 270 MPa | ||
150.0 °C | 250 MPa Show Material materials with Streckgrenze Rp 1,0 of 250 MPa | ||
200.0 °C | 230 MPa Show Material materials with Streckgrenze Rp 1,0 of 230 MPa | ||
250.0 °C | 220 MPa Show Material materials with Streckgrenze Rp 1,0 of 220 MPa | ||
300.0 °C | 210 MPa Show Material materials with Streckgrenze Rp 1,0 of 210 MPa | ||
350.0 °C | 205 MPa Show Material materials with Streckgrenze Rp 1,0 of 205 MPa | ||
400.0 °C | 200 MPa Show Material materials with Streckgrenze Rp 1,0 of 200 MPa | ||
Streckgrenze Rp 1,0, transversal | 20.0 °C | 330 MPa Show Material materials with Streckgrenze Rp 1,0, transversal of 330 MPa | |
Zugfestigkeit | 20.0 °C | 600 - 800 MPa Show Material materials with Zugfestigkeit of 600 - 800 MPa | |
50.0 °C | 581 MPa Show Material materials with Zugfestigkeit of 581 MPa | ||
100.0 °C | 550 MPa Show Material materials with Zugfestigkeit of 550 MPa | ||
150.0 °C | 535 MPa Show Material materials with Zugfestigkeit of 535 MPa | ||
200.0 °C | 520 MPa Show Material materials with Zugfestigkeit of 520 MPa | ||
250.0 °C | 500 MPa Show Material materials with Zugfestigkeit of 500 MPa | ||
300.0 °C | 480 MPa Show Material materials with Zugfestigkeit of 480 MPa | ||
350.0 °C | 475 MPa Show Material materials with Zugfestigkeit of 475 MPa | ||
Zugfestigkeit, transversal | 20.0 °C | 600 - 800 MPa Show Material materials with Zugfestigkeit, transversal of 600 - 800 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.5E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.5E-5 1/K | |
300.0 °C | 1.65E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.65E-5 1/K | ||
Schmelzpunkt | 1230 - 1480 °C Show Material materials with Schmelzpunkt of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Spezifische Wärmekapazität | 20.0 °C | 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 500 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 14 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 14 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 8.5E-7 Ω·m Show Material materials with spezifischer Widerstand of 8.5E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Chrom | 24 - 26 % Show Material materials with Chrom of 24 - 26 % |
Kohlenstoff | 0.02 % Show Material materials with Kohlenstoff of 0.02 % |
Kupfer | 1 - 2 % Show Material materials with Kupfer of 1 - 2 % |
Mangan | 2 % Show Material materials with Mangan of 2 % |
Molybdän | 4.7 - 5.7 % Show Material materials with Molybdän of 4.7 - 5.7 % |
Nickel | 24 - 27 % Show Material materials with Nickel of 24 - 27 % |
Phosphor | 0.03 % Show Material materials with Phosphor of 0.03 % |
Schwefel | 0.01 % Show Material materials with Schwefel of 0.01 % |
Silizium | 0.7 % Show Material materials with Silizium of 0.7 % |
Stickstoff | 0.17 - 0.25 % Show Material materials with Stickstoff of 0.17 - 0.25 % |