Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8 g/cm³ Show Material materials with Dichte of 8 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung A80, transversal | 20.0 °C | 35 - 40 % Show Material materials with Dehnung A80, transversal of 35 - 40 % | |
Dehnung, transversal | 20.0 °C | 35 - 40 % Show Material materials with Dehnung, transversal of 35 - 40 % | |
Elastizitätsmodul | 20.0 °C | 195 GPa Show Material materials with Elastizitätsmodul of 195 GPa | |
100.0 °C | 190 GPa Show Material materials with Elastizitätsmodul of 190 GPa | ||
200.0 °C | 182 GPa Show Material materials with Elastizitätsmodul of 182 GPa | ||
300.0 °C | 174 GPa Show Material materials with Elastizitätsmodul of 174 GPa | ||
400.0 °C | 166 GPa Show Material materials with Elastizitätsmodul of 166 GPa | ||
500.0 °C | 158 GPa Show Material materials with Elastizitätsmodul of 158 GPa | ||
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Austenitic Stainless Steel |
Schubmodule | 23.0 °C | 77 GPa Show Material materials with Schubmodule of 77 GPa | Typical for Austenitic Stainless Steel |
Streckgrenze Rp 0,2 | 50.0 °C | 274 MPa Show Material materials with Streckgrenze Rp 0,2 of 274 MPa | |
100.0 °C | 230 MPa Show Material materials with Streckgrenze Rp 0,2 of 230 MPa | ||
150.0 °C | 205 MPa Show Material materials with Streckgrenze Rp 0,2 of 205 MPa | ||
200.0 °C | 190 MPa Show Material materials with Streckgrenze Rp 0,2 of 190 MPa | ||
250.0 °C | 180 MPa Show Material materials with Streckgrenze Rp 0,2 of 180 MPa | ||
300.0 °C | 170 MPa Show Material materials with Streckgrenze Rp 0,2 of 170 MPa | ||
350.0 °C | 165 MPa Show Material materials with Streckgrenze Rp 0,2 of 165 MPa | ||
400.0 °C | 160 MPa Show Material materials with Streckgrenze Rp 0,2 of 160 MPa | ||
450.0 °C | 153 MPa Show Material materials with Streckgrenze Rp 0,2 of 153 MPa | ||
500.0 °C | 148 MPa Show Material materials with Streckgrenze Rp 0,2 of 148 MPa | ||
Streckgrenze Rp 0,2, transversal | 20.0 °C | 300 - 320 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 300 - 320 MPa | |
Streckgrenze Rp 1,0 | 50.0 °C | 314 MPa Show Material materials with Streckgrenze Rp 1,0 of 314 MPa | |
100.0 °C | 270 MPa Show Material materials with Streckgrenze Rp 1,0 of 270 MPa | ||
150.0 °C | 245 MPa Show Material materials with Streckgrenze Rp 1,0 of 245 MPa | ||
200.0 °C | 225 MPa Show Material materials with Streckgrenze Rp 1,0 of 225 MPa | ||
250.0 °C | 212 MPa Show Material materials with Streckgrenze Rp 1,0 of 212 MPa | ||
300.0 °C | 200 MPa Show Material materials with Streckgrenze Rp 1,0 of 200 MPa | ||
350.0 °C | 195 MPa Show Material materials with Streckgrenze Rp 1,0 of 195 MPa | ||
400.0 °C | 190 MPa Show Material materials with Streckgrenze Rp 1,0 of 190 MPa | ||
450.0 °C | 184 MPa Show Material materials with Streckgrenze Rp 1,0 of 184 MPa | ||
500.0 °C | 180 MPa Show Material materials with Streckgrenze Rp 1,0 of 180 MPa | ||
Streckgrenze Rp 1,0, transversal | 20.0 °C | 340 - 350 MPa Show Material materials with Streckgrenze Rp 1,0, transversal of 340 - 350 MPa | |
Zugfestigkeit | 20.0 °C | 650 - 850 MPa Show Material materials with Zugfestigkeit of 650 - 850 MPa | |
50.0 °C | 637 MPa Show Material materials with Zugfestigkeit of 637 MPa | ||
100.0 °C | 615 MPa Show Material materials with Zugfestigkeit of 615 MPa | ||
150.0 °C | 587 MPa Show Material materials with Zugfestigkeit of 587 MPa | ||
200.0 °C | 560 MPa Show Material materials with Zugfestigkeit of 560 MPa | ||
250.0 °C | 542 MPa Show Material materials with Zugfestigkeit of 542 MPa | ||
300.0 °C | 525 MPa Show Material materials with Zugfestigkeit of 525 MPa | ||
350.0 °C | 517 MPa Show Material materials with Zugfestigkeit of 517 MPa | ||
400.0 °C | 510 MPa Show Material materials with Zugfestigkeit of 510 MPa | ||
450.0 °C | 502 MPa Show Material materials with Zugfestigkeit of 502 MPa | ||
500.0 °C | 495 MPa Show Material materials with Zugfestigkeit of 495 MPa | ||
Zugfestigkeit, transversal | 20.0 °C | 650 - 850 MPa Show Material materials with Zugfestigkeit, transversal of 650 - 850 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.65E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.65E-5 1/K | |
200.0 °C | 1.7E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 1/K | ||
300.0 °C | 1.75E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.75E-5 1/K | ||
400.0 °C | 1.8E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.8E-5 1/K | ||
500.0 °C | 1.8E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.8E-5 1/K | ||
Schmelzpunkt | 1230 - 1480 °C Show Material materials with Schmelzpunkt of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Spezifische Wärmekapazität | 20.0 °C | 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 500 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 14 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 14 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 8.5E-7 Ω·m Show Material materials with spezifischer Widerstand of 8.5E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Chrom | 19.5 - 20.5 % Show Material materials with Chrom of 19.5 - 20.5 % |
Kohlenstoff | 0.02 % Show Material materials with Kohlenstoff of 0.02 % |
Kupfer | 0.5 - 1 % Show Material materials with Kupfer of 0.5 - 1 % |
Mangan | 1 % Show Material materials with Mangan of 1 % |
Molybdän | 6 - 7 % Show Material materials with Molybdän of 6 - 7 % |
Nickel | 17.5 - 18.5 % Show Material materials with Nickel of 17.5 - 18.5 % |
Phosphor | 0.03 % Show Material materials with Phosphor of 0.03 % |
Schwefel | 0.01 % Show Material materials with Schwefel of 0.01 % |
Silizium | 0.7 % Show Material materials with Silizium of 0.7 % |
Stickstoff | 0.18 - 0.25 % Show Material materials with Stickstoff of 0.18 - 0.25 % |