Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8 g/cm³ Show Material materials with Dichte of 8 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 35 % Show Material materials with Dehnung of 35 % | |
Elastizitätsmodul | 20.0 °C | 191 GPa Show Material materials with Elastizitätsmodul of 191 GPa | |
Härte, Brinell | 20.0 °C | 223 [-] Show Material materials with Härte, Brinell of 223 [-] | |
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Austenitic Stainless Steel |
Schubmodule | 23.0 °C | 77 GPa Show Material materials with Schubmodule of 77 GPa | Typical for Austenitic Stainless Steel |
Streckgrenze Rp 0,2 | 20.0 °C | 180 MPa Show Material materials with Streckgrenze Rp 0,2 of 180 MPa | |
Streckgrenze Rp 1,0 | 20.0 °C | 220 MPa Show Material materials with Streckgrenze Rp 1,0 of 220 MPa | |
Zugfestigkeit | 20.0 °C | 500 - 750 MPa Show Material materials with Zugfestigkeit of 500 - 750 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 200.0 °C | 1.55E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.55E-5 1/K | |
400.0 °C | 1.65E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.65E-5 1/K | ||
600.0 °C | 1.65E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.65E-5 1/K | ||
800.0 °C | 1.77E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.77E-5 1/K | ||
1000.0 °C | 1.84E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.84E-5 1/K | ||
Max. Betriebstemperatur, lang | -10 - 1000 °C Show Material materials with Max. Betriebstemperatur, lang of -10 - 1000 °C | ||
Schmelzpunkt | 1230 - 1480 °C Show Material materials with Schmelzpunkt of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Spezifische Wärmekapazität | 20.0 °C | 450 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 450 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 12 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 12 W/(m·K) | |
500.0 °C | 20 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 20 W/(m·K) | ||
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 9.6E-7 Ω·m Show Material materials with spezifischer Widerstand of 9.6E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.025 % Show Material materials with Aluminium of 0.025 % |
Cerium | 0.05 - 0.1 % Show Material materials with Cerium of 0.05 - 0.1 % |
Chrom | 26 - 28 % Show Material materials with Chrom of 26 - 28 % |
Kohlenstoff | 0.04 - 0.08 % Show Material materials with Kohlenstoff of 0.04 - 0.08 % |
Mangan | 1 % Show Material materials with Mangan of 1 % |
Nickel | 31 - 33 % Show Material materials with Nickel of 31 - 33 % |
Niobium | 0.6 - 1 % Show Material materials with Niobium of 0.6 - 1 % |
Phosphor | 0.02 % Show Material materials with Phosphor of 0.02 % |
Schwefel | 0.01 % Show Material materials with Schwefel of 0.01 % |
Silizium | 0.3 % Show Material materials with Silizium of 0.3 % |
Stickstoff | 0.11 % Show Material materials with Stickstoff of 0.11 % |