Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 7.8 - 7.9 g/cm³ Show Material materials with Dichte of 7.8 - 7.9 g/cm³ | Typical for Chromium Molybdenum Steel |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 20 % Show Material materials with Dehnung of 20 % | |
Dehnung, transversal | 20.0 °C | 18 % Show Material materials with Dehnung, transversal of 18 % | |
Elastizitätsmodul | 23.0 °C | 200 - 215 GPa Show Material materials with Elastizitätsmodul of 200 - 215 GPa | Typical for Chromium Molybdenum Steel |
Poissonzahl | 23.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Chromium Molybdenum Steel |
Streckgrenze Rp 0,2 | 20.0 °C | 355 MPa Show Material materials with Streckgrenze Rp 0,2 of 355 MPa | |
100.0 °C | 323 MPa Show Material materials with Streckgrenze Rp 0,2 of 323 MPa | ||
150.0 °C | 312 MPa Show Material materials with Streckgrenze Rp 0,2 of 312 MPa | ||
200.0 °C | 304 MPa Show Material materials with Streckgrenze Rp 0,2 of 304 MPa | ||
250.0 °C | 296 MPa Show Material materials with Streckgrenze Rp 0,2 of 296 MPa | ||
300.0 °C | 289 MPa Show Material materials with Streckgrenze Rp 0,2 of 289 MPa | ||
350.0 °C | 280 MPa Show Material materials with Streckgrenze Rp 0,2 of 280 MPa | ||
400.0 °C | 275 MPa Show Material materials with Streckgrenze Rp 0,2 of 275 MPa | ||
450.0 °C | 257 MPa Show Material materials with Streckgrenze Rp 0,2 of 257 MPa | ||
500.0 °C | 239 MPa Show Material materials with Streckgrenze Rp 0,2 of 239 MPa | ||
Streckgrenze Rp 0,2, transversal | 20.0 °C | 355 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 355 MPa | |
Zugfestigkeit | 20.0 °C | 540 - 680 MPa Show Material materials with Zugfestigkeit of 540 - 680 MPa | |
Zugfestigkeit, transversal | 20.0 °C | 540 - 680 MPa Show Material materials with Zugfestigkeit, transversal of 540 - 680 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.1E-5 - 1.4E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.1E-5 - 1.4E-5 1/K | Typical for Chromium Molybdenum Steel |
Max. Betriebstemperatur, lang | 200 - 550 °C Show Material materials with Max. Betriebstemperatur, lang of 200 - 550 °C | ||
Schmelzpunkt | 1382 - 1529 °C Show Material materials with Schmelzpunkt of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Spezifische Wärmekapazität | 23.0 °C | 448 - 502 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 448 - 502 J/(kg·K) | Typical for Chromium Molybdenum Steel |
Wärmeleitfähigkeit | 23.0 °C | 36 - 43 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36 - 43 W/(m·K) | Typical for Chromium Molybdenum Steel |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.04 % Show Material materials with Aluminium of 0.04 % |
Chrom | 2 - 2.5 % Show Material materials with Chrom of 2 - 2.5 % |
Kohlenstoff | 0.08 - 0.15 % Show Material materials with Kohlenstoff of 0.08 - 0.15 % |
Kupfer | 0.3 % Show Material materials with Kupfer of 0.3 % |
Mangan | 0.4 - 0.8 % Show Material materials with Mangan of 0.4 - 0.8 % |
Molybdän | 0.9 - 1.1 % Show Material materials with Molybdän of 0.9 - 1.1 % |
Nickel | 0.3 % Show Material materials with Nickel of 0.3 % |
Phosphor | 0.03 % Show Material materials with Phosphor of 0.03 % |
Schwefel | 0.01 - 0.02 % Show Material materials with Schwefel of 0.01 - 0.02 % |
Silizium | 0.5 % Show Material materials with Silizium of 0.5 % |