Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung | 20.0 °C | 20 % Show Material materials with Dehnung of 20 % |
Dehnung, transversal | 20.0 °C | 18 % Show Material materials with Dehnung, transversal of 18 % |
Streckgrenze Rp 0,2 | 20.0 °C | 510 MPa Show Material materials with Streckgrenze Rp 0,2 of 510 MPa |
100.0 °C | 370 MPa Show Material materials with Streckgrenze Rp 0,2 of 370 MPa | |
200.0 °C | 335 MPa Show Material materials with Streckgrenze Rp 0,2 of 335 MPa | |
250.0 °C | 315 MPa Show Material materials with Streckgrenze Rp 0,2 of 315 MPa | |
300.0 °C | 300 MPa Show Material materials with Streckgrenze Rp 0,2 of 300 MPa | |
Streckgrenze Rp 0,2, transversal | 20.0 °C | 510 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 510 MPa |
Zugfestigkeit | 20.0 °C | 690 - 840 MPa Show Material materials with Zugfestigkeit of 690 - 840 MPa |
Zugfestigkeit, transversal | 20.0 °C | 690 - 840 MPa Show Material materials with Zugfestigkeit, transversal of 690 - 840 MPa |
Chemical properties
Property | Value |
---|---|
Kohlenstoff | 0.13 % Show Material materials with Kohlenstoff of 0.13 % |
Kupfer | 0.3 % Show Material materials with Kupfer of 0.3 % |
Mangan | 0.3 - 0.8 % Show Material materials with Mangan of 0.3 - 0.8 % |
Molybdän | 0.1 % Show Material materials with Molybdän of 0.1 % |
Nickel | 8.5 - 9.5 % Show Material materials with Nickel of 8.5 - 9.5 % |
Phosphor | 0.02 % Show Material materials with Phosphor of 0.02 % |
Schwefel | 0.005 - 0.01 % Show Material materials with Schwefel of 0.005 - 0.01 % |
Silizium | 0.15 - 0.35 % Show Material materials with Silizium of 0.15 - 0.35 % |
Vanadium | 0.05 % Show Material materials with Vanadium of 0.05 % |