Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8 g/cm³ Show Material materials with Dichte of 8 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 40 % Show Material materials with Dehnung of 40 % | |
Dehnung, transversal | 20.0 °C | 30 % Show Material materials with Dehnung, transversal of 30 % | |
Elastizitätsmodul | 20.0 °C | 200 GPa Show Material materials with Elastizitätsmodul of 200 GPa | |
100.0 °C | 194 GPa Show Material materials with Elastizitätsmodul of 194 GPa | ||
200.0 °C | 186 GPa Show Material materials with Elastizitätsmodul of 186 GPa | ||
300.0 °C | 179 GPa Show Material materials with Elastizitätsmodul of 179 GPa | ||
400.0 °C | 172 GPa Show Material materials with Elastizitätsmodul of 172 GPa | ||
500.0 °C | 165 GPa Show Material materials with Elastizitätsmodul of 165 GPa | ||
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Austenitic Stainless Steel |
Schubmodule | 23.0 °C | 77 GPa Show Material materials with Schubmodule of 77 GPa | Typical for Austenitic Stainless Steel |
Streckgrenze Rp 0,2 | 20.0 °C | 205 MPa Show Material materials with Streckgrenze Rp 0,2 of 205 MPa | |
50.0 °C | 195 MPa Show Material materials with Streckgrenze Rp 0,2 of 195 MPa | ||
100.0 °C | 175 MPa Show Material materials with Streckgrenze Rp 0,2 of 175 MPa | ||
150.0 °C | 158 MPa Show Material materials with Streckgrenze Rp 0,2 of 158 MPa | ||
200.0 °C | 145 MPa Show Material materials with Streckgrenze Rp 0,2 of 145 MPa | ||
250.0 °C | 135 MPa Show Material materials with Streckgrenze Rp 0,2 of 135 MPa | ||
300.0 °C | 127 MPa Show Material materials with Streckgrenze Rp 0,2 of 127 MPa | ||
350.0 °C | 120 MPa Show Material materials with Streckgrenze Rp 0,2 of 120 MPa | ||
400.0 °C | 115 MPa Show Material materials with Streckgrenze Rp 0,2 of 115 MPa | ||
450.0 °C | 112 MPa Show Material materials with Streckgrenze Rp 0,2 of 112 MPa | ||
500.0 °C | 110 MPa Show Material materials with Streckgrenze Rp 0,2 of 110 MPa | ||
550.0 °C | 108 MPa Show Material materials with Streckgrenze Rp 0,2 of 108 MPa | ||
Streckgrenze Rp 0,2, transversal | 20.0 °C | 205 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 205 MPa | |
Streckgrenze Rp 1,0 | 20.0 °C | 240 MPa Show Material materials with Streckgrenze Rp 1,0 of 240 MPa | |
50.0 °C | 228 MPa Show Material materials with Streckgrenze Rp 1,0 of 228 MPa | ||
100.0 °C | 210 MPa Show Material materials with Streckgrenze Rp 1,0 of 210 MPa | ||
150.0 °C | 190 MPa Show Material materials with Streckgrenze Rp 1,0 of 190 MPa | ||
200.0 °C | 175 MPa Show Material materials with Streckgrenze Rp 1,0 of 175 MPa | ||
250.0 °C | 165 MPa Show Material materials with Streckgrenze Rp 1,0 of 165 MPa | ||
300.0 °C | 155 MPa Show Material materials with Streckgrenze Rp 1,0 of 155 MPa | ||
350.0 °C | 150 MPa Show Material materials with Streckgrenze Rp 1,0 of 150 MPa | ||
400.0 °C | 145 MPa Show Material materials with Streckgrenze Rp 1,0 of 145 MPa | ||
450.0 °C | 141 MPa Show Material materials with Streckgrenze Rp 1,0 of 141 MPa | ||
500.0 °C | 139 MPa Show Material materials with Streckgrenze Rp 1,0 of 139 MPa | ||
550.0 °C | 137 MPa Show Material materials with Streckgrenze Rp 1,0 of 137 MPa | ||
Streckgrenze Rp 1,0, transversal | 20.0 °C | 240 MPa Show Material materials with Streckgrenze Rp 1,0, transversal of 240 MPa | |
Zugfestigkeit | 20.0 °C | 510 - 710 MPa Show Material materials with Zugfestigkeit of 510 - 710 MPa | |
Zugfestigkeit, transversal | 20.0 °C | 510 - 710 MPa Show Material materials with Zugfestigkeit, transversal of 510 - 710 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.6E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6E-5 1/K | |
200.0 °C | 1.65E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.65E-5 1/K | ||
300.0 °C | 1.7E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.7E-5 1/K | ||
400.0 °C | 1.75E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.75E-5 1/K | ||
500.0 °C | 1.8E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.8E-5 1/K | ||
Schmelzpunkt | 1230 - 1480 °C Show Material materials with Schmelzpunkt of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Spezifische Wärmekapazität | 20.0 °C | 500 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 500 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 15 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 15 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 7.5E-7 Ω·m Show Material materials with spezifischer Widerstand of 7.5E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Chrom | 16.5 - 18.5 % Show Material materials with Chrom of 16.5 - 18.5 % |
Kohlenstoff | 0.05 % Show Material materials with Kohlenstoff of 0.05 % |
Mangan | 2 % Show Material materials with Mangan of 2 % |
Molybdän | 2.5 - 3 % Show Material materials with Molybdän of 2.5 - 3 % |
Nickel | 10.5 - 13 % Show Material materials with Nickel of 10.5 - 13 % |
Phosphor | 0.04 % Show Material materials with Phosphor of 0.04 % |
Schwefel | 0.015 % Show Material materials with Schwefel of 0.015 % |
Silizium | 1 % Show Material materials with Silizium of 1 % |
Stickstoff | 0.11 % Show Material materials with Stickstoff of 0.11 % |