Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 8 g/cm³ Show Material materials with Dichte of 8 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 35 % Show Material materials with Dehnung of 35 % | |
Dehnung, transversal | 20.0 °C | 30 % Show Material materials with Dehnung, transversal of 30 % | |
Elastizitätsmodul | 20.0 °C | 207 GPa Show Material materials with Elastizitätsmodul of 207 GPa | |
100.0 °C | 201 GPa Show Material materials with Elastizitätsmodul of 201 GPa | ||
200.0 °C | 193 GPa Show Material materials with Elastizitätsmodul of 193 GPa | ||
300.0 °C | 184 GPa Show Material materials with Elastizitätsmodul of 184 GPa | ||
400.0 °C | 175 GPa Show Material materials with Elastizitätsmodul of 175 GPa | ||
500.0 °C | 165 GPa Show Material materials with Elastizitätsmodul of 165 GPa | ||
600.0 °C | 158 GPa Show Material materials with Elastizitätsmodul of 158 GPa | ||
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Austenitic Stainless Steel |
Schubmodule | 23.0 °C | 77 GPa Show Material materials with Schubmodule of 77 GPa | Typical for Austenitic Stainless Steel |
Streckgrenze Rp 0,2 | 20.0 °C | 220 MPa Show Material materials with Streckgrenze Rp 0,2 of 220 MPa | |
50.0 °C | 213 MPa Show Material materials with Streckgrenze Rp 0,2 of 213 MPa | ||
100.0 °C | 188 MPa Show Material materials with Streckgrenze Rp 0,2 of 188 MPa | ||
150.0 °C | 171 MPa Show Material materials with Streckgrenze Rp 0,2 of 171 MPa | ||
200.0 °C | 161 MPa Show Material materials with Streckgrenze Rp 0,2 of 161 MPa | ||
250.0 °C | 153 MPa Show Material materials with Streckgrenze Rp 0,2 of 153 MPa | ||
300.0 °C | 148 MPa Show Material materials with Streckgrenze Rp 0,2 of 148 MPa | ||
350.0 °C | 145 MPa Show Material materials with Streckgrenze Rp 0,2 of 145 MPa | ||
400.0 °C | 144 MPa Show Material materials with Streckgrenze Rp 0,2 of 144 MPa | ||
450.0 °C | 141 MPa Show Material materials with Streckgrenze Rp 0,2 of 141 MPa | ||
500.0 °C | 139 MPa Show Material materials with Streckgrenze Rp 0,2 of 139 MPa | ||
550.0 °C | 136 MPa Show Material materials with Streckgrenze Rp 0,2 of 136 MPa | ||
Streckgrenze Rp 0,2, transversal | 20.0 °C | 220 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 220 MPa | |
Streckgrenze Rp 1,0 | 20.0 °C | 270 MPa Show Material materials with Streckgrenze Rp 1,0 of 270 MPa | |
50.0 °C | 254 MPa Show Material materials with Streckgrenze Rp 1,0 of 254 MPa | ||
100.0 °C | 232 MPa Show Material materials with Streckgrenze Rp 1,0 of 232 MPa | ||
150.0 °C | 210 MPa Show Material materials with Streckgrenze Rp 1,0 of 210 MPa | ||
200.0 °C | 195 MPa Show Material materials with Streckgrenze Rp 1,0 of 195 MPa | ||
250.0 °C | 190 MPa Show Material materials with Streckgrenze Rp 1,0 of 190 MPa | ||
300.0 °C | 187 MPa Show Material materials with Streckgrenze Rp 1,0 of 187 MPa | ||
350.0 °C | 184 MPa Show Material materials with Streckgrenze Rp 1,0 of 184 MPa | ||
400.0 °C | 182 MPa Show Material materials with Streckgrenze Rp 1,0 of 182 MPa | ||
450.0 °C | 179 MPa Show Material materials with Streckgrenze Rp 1,0 of 179 MPa | ||
500.0 °C | 178 MPa Show Material materials with Streckgrenze Rp 1,0 of 178 MPa | ||
550.0 °C | 175 MPa Show Material materials with Streckgrenze Rp 1,0 of 175 MPa | ||
Streckgrenze Rp 1,0, transversal | 20.0 °C | 270 MPa Show Material materials with Streckgrenze Rp 1,0, transversal of 270 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.57E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.57E-5 1/K | |
200.0 °C | 1.68E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.68E-5 1/K | ||
300.0 °C | 1.77E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.77E-5 1/K | ||
400.0 °C | 1.83E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.83E-5 1/K | ||
500.0 °C | 1.86E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.86E-5 1/K | ||
600.0 °C | 1.9E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.9E-5 1/K | ||
Schmelzpunkt | 1230 - 1480 °C Show Material materials with Schmelzpunkt of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Spezifische Wärmekapazität | 20.0 °C | 480 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 480 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 12.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 12.5 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 7.4E-7 Ω·m Show Material materials with spezifischer Widerstand of 7.4E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Bor | 3E-3 - 9E-3 % Show Material materials with Bor of 3E-3 - 9E-3 % |
Chrom | 14 - 16 % Show Material materials with Chrom of 14 - 16 % |
Kohlenstoff | 0.06 - 0.15 % Show Material materials with Kohlenstoff of 0.06 - 0.15 % |
Mangan | 5.5 - 7 % Show Material materials with Mangan of 5.5 - 7 % |
Molybdän | 0.8 - 1.2 % Show Material materials with Molybdän of 0.8 - 1.2 % |
Nickel | 9 - 11 % Show Material materials with Nickel of 9 - 11 % |
Niobium | 0.75 - 1.25 % Show Material materials with Niobium of 0.75 - 1.25 % |
Phosphor | 0.04 % Show Material materials with Phosphor of 0.04 % |
Schwefel | 0.015 % Show Material materials with Schwefel of 0.015 % |
Silizium | 0.2 - 1 % Show Material materials with Silizium of 0.2 - 1 % |
Stickstoff | 0.06 - 0.14 % Show Material materials with Stickstoff of 0.06 - 0.14 % |
Vanadium | 0.15 - 0.4 % Show Material materials with Vanadium of 0.15 - 0.4 % |