Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 7.84 g/cm³ Show Material materials with Dichte of 7.84 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 11 % Show Material materials with Dehnung of 11 % | |
Elastizitätsmodul | 20.0 °C | 210 GPa Show Material materials with Elastizitätsmodul of 210 GPa | |
Poissonzahl | 23.0 °C | 0.3 [-] Show Material materials with Poissonzahl of 0.3 [-] | Typical for Steel |
Streckgrenze | 20.0 °C | 830 - 890 MPa Show Material materials with Streckgrenze of 830 - 890 MPa | |
Zugfestigkeit | 20.0 °C | 880 - 1100 MPa Show Material materials with Zugfestigkeit of 880 - 1100 MPa |
Thermisch
Property | Temperature | Value |
---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.2E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.2E-5 1/K |
Spezifische Wärmekapazität | 20.0 °C | 440 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 440 J/(kg·K) |
Wärmeleitfähigkeit | 20.0 °C | 38 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 38 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 2.8E-7 Ω·m Show Material materials with spezifischer Widerstand of 2.8E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Bor | 5E-3 % Show Material materials with Bor of 5E-3 % |
Chrom | 1.5 % Show Material materials with Chrom of 1.5 % |
Kohlenstoff | 0.2 % Show Material materials with Kohlenstoff of 0.2 % |
Kupfer | 0.5 % Show Material materials with Kupfer of 0.5 % |
Mangan | 1.7 % Show Material materials with Mangan of 1.7 % |
Molybdän | 0.7 % Show Material materials with Molybdän of 0.7 % |
Nickel | 2 % Show Material materials with Nickel of 2 % |
Niobium | 0.06 % Show Material materials with Niobium of 0.06 % |
Phosphor | 0.02 % Show Material materials with Phosphor of 0.02 % |
Schwefel | 0.01 % Show Material materials with Schwefel of 0.01 % |
Silizium | 0.8 % Show Material materials with Silizium of 0.8 % |
Stickstoff | 0.02 % Show Material materials with Stickstoff of 0.02 % |
Titan | 0.05 % Show Material materials with Titan of 0.05 % |
Vanadium | 0.12 % Show Material materials with Vanadium of 0.12 % |
Zirkonium | 0.15 % Show Material materials with Zirkonium of 0.15 % |