Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 7.8 - 7.9 g/cm³ Show Material materials with Dichte of 7.8 - 7.9 g/cm³ | Typical for Chromium Molybdenum Steel |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 16 % Show Material materials with Dehnung of 16 % | |
Elastizitätsmodul | 23.0 °C | 200 - 215 GPa Show Material materials with Elastizitätsmodul of 200 - 215 GPa | Typical for Chromium Molybdenum Steel |
Flächenreduzierung | 20.0 °C | 50 % Show Material materials with Flächenreduzierung of 50 % | |
Poissonzahl | 23.0 °C | 0.29 [-] Show Material materials with Poissonzahl of 0.29 [-] | Typical for Chromium Molybdenum Steel |
Streckgrenze Rp 0,2 | 20.0 °C | 640 - 700 MPa Show Material materials with Streckgrenze Rp 0,2 of 640 - 700 MPa | |
50.0 °C | 625 - 681 MPa Show Material materials with Streckgrenze Rp 0,2 of 625 - 681 MPa | ||
100.0 °C | 605 - 662 MPa Show Material materials with Streckgrenze Rp 0,2 of 605 - 662 MPa | ||
150.0 °C | 584 - 639 MPa Show Material materials with Streckgrenze Rp 0,2 of 584 - 639 MPa | ||
200.0 °C | 563 - 616 MPa Show Material materials with Streckgrenze Rp 0,2 of 563 - 616 MPa | ||
250.0 °C | 549 - 601 MPa Show Material materials with Streckgrenze Rp 0,2 of 549 - 601 MPa | ||
300.0 °C | 535 - 585 MPa Show Material materials with Streckgrenze Rp 0,2 of 535 - 585 MPa | ||
350.0 °C | 521 - 570 MPa Show Material materials with Streckgrenze Rp 0,2 of 521 - 570 MPa | ||
400.0 °C | 500 - 547 MPa Show Material materials with Streckgrenze Rp 0,2 of 500 - 547 MPa | ||
450.0 °C | 472 - 516 MPa Show Material materials with Streckgrenze Rp 0,2 of 472 - 516 MPa | ||
500.0 °C | 422 - 462 MPa Show Material materials with Streckgrenze Rp 0,2 of 422 - 462 MPa | ||
550.0 °C | 331 - 362 MPa Show Material materials with Streckgrenze Rp 0,2 of 331 - 362 MPa | ||
600.0 °C | 204 - 223 MPa Show Material materials with Streckgrenze Rp 0,2 of 204 - 223 MPa | ||
Zugfestigkeit | 20.0 °C | 850 - 1060 MPa Show Material materials with Zugfestigkeit of 850 - 1060 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.1E-5 - 1.4E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.1E-5 - 1.4E-5 1/K | Typical for Chromium Molybdenum Steel |
Schmelzpunkt | 1382 - 1529 °C Show Material materials with Schmelzpunkt of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Spezifische Wärmekapazität | 23.0 °C | 448 - 502 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 448 - 502 J/(kg·K) | Typical for Chromium Molybdenum Steel |
Wärmeleitfähigkeit | 23.0 °C | 36 - 43 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 36 - 43 W/(m·K) | Typical for Chromium Molybdenum Steel |
Chemical properties
Property | Value |
---|---|
Chrom | 1.2 - 1.5 % Show Material materials with Chrom of 1.2 - 1.5 % |
Kohlenstoff | 0.39 - 0.45 % Show Material materials with Kohlenstoff of 0.39 - 0.45 % |
Mangan | 0.4 - 0.7 % Show Material materials with Mangan of 0.4 - 0.7 % |
Molybdän | 0.5 - 0.7 % Show Material materials with Molybdän of 0.5 - 0.7 % |
Phosphor | 0.03 - 0.04 % Show Material materials with Phosphor of 0.03 - 0.04 % |
Schwefel | 0.035 % Show Material materials with Schwefel of 0.035 % |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % |