Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung A5 | 20.0 °C | 17 % Show Material materials with Dehnung A5 of 17 % |
Schlagfestigkeit, Charpy gekerbt | -20.0 °C | 39 kJ/m² Show Material materials with Schlagfestigkeit, Charpy gekerbt of 39 kJ/m² |
Streckgrenze Rp 0,2 | 20.0 °C | 380 - 460 MPa Show Material materials with Streckgrenze Rp 0,2 of 380 - 460 MPa |
Zugfestigkeit | 20.0 °C | 510 - 720 MPa Show Material materials with Zugfestigkeit of 510 - 720 MPa |
impactTransVNotch | -20.0 °C | 21 kJ/m² Show Material materials with impactTransVNotch of 21 kJ/m² |
Chemical properties
Property | Value |
---|---|
Aluminium | 0 - 0.02 % Show Material materials with Aluminium of 0 - 0.02 % |
Bor | 0 - 5E-3 % Show Material materials with Bor of 0 - 5E-3 % |
Chrom | 0.7 - 2 % Show Material materials with Chrom of 0.7 - 2 % |
Eisen | 90.44 - 99.3 % Show Material materials with Eisen of 90.44 - 99.3 % |
Kohlenstoff | 0.2 % Show Material materials with Kohlenstoff of 0.2 % |
Kupfer | 0.7 - 1.5 % Show Material materials with Kupfer of 0.7 - 1.5 % |
Mangan | 0.7 - 1.7 % Show Material materials with Mangan of 0.7 - 1.7 % |
Molybdän | 0.4 - 1 % Show Material materials with Molybdän of 0.4 - 1 % |
Nickel | 1 - 2 % Show Material materials with Nickel of 1 - 2 % |
Niobium | 0 - 0.06 % Show Material materials with Niobium of 0 - 0.06 % |
Phosphor | 0.03 - 0.04 % Show Material materials with Phosphor of 0.03 - 0.04 % |
Schwefel | 0.03 - 0.035 % Show Material materials with Schwefel of 0.03 - 0.035 % |
Silizium | 0.5 - 0.55 % Show Material materials with Silizium of 0.5 - 0.55 % |
Stickstoff | 0 - 0.02 % Show Material materials with Stickstoff of 0 - 0.02 % |
Titan | 0 - 0.2 % Show Material materials with Titan of 0 - 0.2 % |
Vanadium | 0 - 0.2 % Show Material materials with Vanadium of 0 - 0.2 % |
Zirkonium | 0 - 0.15 % Show Material materials with Zirkonium of 0 - 0.15 % |
Technological properties
Property | ||
---|---|---|
Processing history | normalized, controlled rolled |